Material Overview
GH5188, also written GH188, is a cobalt base wrought alloy supplied as bar and forged stock for high-temperature components. The grade is designated in the wrought superalloy series covered by GB/T 14992, which classifies and designates high temperature materials. The alloy is solid solution strengthened rather than precipitation hardened: chromium provides oxidation and corrosion resistance, tungsten and nickel contribute solid solution strengthening, and a small lanthanum addition improves the adherence of the protective oxide scale at high temperature.
Because the strengthening mechanism does not depend on a precipitation reaction, the alloy keeps useful strength at temperatures where precipitation hardened alloys would overage and soften. That characteristic is the reason the grade appears in combustion and turbine components that see continuous high temperature exposure.
Composition and Key Characteristics
| Element | Typical content (percent by mass) |
|---|---|
| Cobalt | Balance |
| Chromium | 20.0-24.0 |
| Nickel | 20.0-24.0 |
| Tungsten | 13.0-16.0 |
| Iron | 3.0 max |
| Manganese | 1.25 max |
| Silicon | 0.20-0.50 |
| Lanthanum | Small controlled addition |
The lanthanum addition improves the adherence of the protective oxide scale at high temperature, which is one of the reasons the grade performs well in continuous high temperature service.
Excellent oxidation resistance in continuous high temperature service
Good strength retention without a precipitation hardening reaction
Satisfactory fatigue performance under thermal cycling
Resistance to hot corrosion in combustion environments
Applications
The cast and wrought forms of the grade are used across a family of hot section components, and bar product is machined into parts that must hold their shape and strength at temperature.
Turbine blades, where high temperature strength, fatigue resistance and corrosion resistance are all required
Combustion chamber components, including combustion chamber liners and spark plugs, which must withstand hot pressurised combustion gas
High-temperature seals such as turbine covers and sealing rings, which must keep their sealing performance under thermal cycling
Other hot section parts of engines and industrial furnaces
Processing and Fabrication
The alloy is hot worked within a controlled temperature range and finished by machining to the required geometry. Because it is solid solution strengthened, the final properties are obtained by solution treatment followed by controlled cooling, and the treatment is carried out so as to produce a uniform grain structure. Machining requires sharp tooling and appropriate cutting parameters, since the alloy work hardens rapidly and generates heat at the cutting edge.
Welding is possible with processes and consumables suited to the grade, and preheat is not normally required. Components that have been formed or welded are stress relieved or solution treated as specified by the design, and the heat treatment is recorded for traceability. Careful control of surface finish matters for sealing surfaces and for components subject to fatigue loading, because machining marks act as initiation sites for cracks.
Quality Control and Delivery
Bars are supplied in the solution treated condition, or in a condition specified in the order, with a certificate recording the heat number, chemical analysis, heat treatment and mechanical test results. Tensile testing is carried out in accordance with GB/T 228.1, hardness is measured on the finished product, and ultrasonic testing can be specified to verify internal soundness. Dimensional inspection covers diameter, length, straightness and surface condition, and non-destructive examination results are recorded for the components supplied to the customer. Typical industry stock ranges cover a selection of diameters, and non-standard sizes are produced to order.
Frequently Asked Questions
Q: Is GH5188 the same as GH188?
A: Yes. GH5188 and GH188 refer to the same cobalt base wrought alloy grade, and the two designations are used interchangeably in technical documents.
Q: How is GH5188 strengthened?
A: It is strengthened by solid solution hardening through tungsten, chromium and nickel additions rather than by a precipitation hardening reaction.
Q: What is the main advantage of the grade?
A: It retains useful strength and resists oxidation at high temperature, which makes it suitable for continuous high temperature service in combustion and turbine components.
Q: Where is the alloy used?
A: In turbine blades, combustion chamber liners and spark plugs, and in high-temperature seals such as turbine covers and sealing rings.
Q: How are the mechanical properties verified?
A: By tensile testing in accordance with GB/T 228.1 and by hardness testing, with the results recorded on the material certificate.
Q: Which standard designates the grade?
A: The grade is designated within the wrought superalloy series covered by GB/T 14992.