GH5188 Alloy Bar Mechanical Properties and Test Methods

Feb 22, 2024 Leave a message

How the Property Level Is Set

GH5188 is a cobalt base wrought alloy whose mechanical properties depend on the delivered condition rather than on composition alone. The grade is solid solution strengthened, so a solution treated bar has a moderate strength level with high ductility, while a bar that has been cold worked and aged develops a much higher strength level with correspondingly lower elongation. This is why a property table for the grade must always state the condition to which the values apply.

The grade is designated in the wrought superalloy series covered by GB/T 14992. Mechanical testing is carried out in accordance with GB/T 228.1 for tensile properties at room temperature, with hardness measured on the finished product.

Mechanical Properties by Condition

Property Cold worked and aged condition
Yield strength Approximately 690 MPa to 1035 MPa
Tensile strength Generally above 1200 MPa
Elongation Typically below 15 percent
Hardness Approximately 30 to 40 HRC

The spread in the yield strength range reflects the degree of cold work and the aging treatment applied, together with the precise composition of the heat. A bar ordered to the upper end of the strength range carries less ductility than one ordered to the lower end, and the two are not interchangeable in a design that depends on either property.

Property Balance and Design Consequences

High strength combined with moderate ductility in the cold worked and aged condition

Better formability and weldability in the solution treated condition, at a lower strength level

Strength retention at high temperature because the alloy is solid solution strengthened

Hardness values in the 30 to 40 HRC band indicate the need for appropriate machining practice

When a component is designed around the high strength condition, the fabrication sequence must be planned so that forming and machining operations are completed before the final aging treatment, because the aged bar is much less forgiving of bending and cutting forces. Conversely, where a component is welded, the joint may need a post-weld solution treatment to restore ductility in the heat affected zone.

Test Methods and Sampling

Tensile testing is carried out at room temperature in accordance with GB/T 228.1, using specimens machined from the bar in the delivered condition and orientation. Hardness is measured on the finished bar, and Rockwell C values in the 30 to 40 range correspond to the high strength condition reported above. Where the order requires elevated temperature properties, additional tests are carried out at the agreed temperature, and the results are listed separately on the certificate. Grain size examination is commonly specified together with the mechanical tests, because grain structure influences both strength and fatigue behaviour.

Supply Condition and Traceability

Bar is supplied in the condition stated in the order, commonly solution treated or cold worked and aged, with a certificate recording the heat number, chemical analysis, heat treatment, tensile results and hardness. Dimensional inspection covers diameter, length, straightness and surface finish, and ultrasonic testing can be ordered to confirm internal soundness of the bar before machining. Surface defects such as seams and laps are removed by grinding within the permitted depth, and the removal is recorded so that the finished part remains within the drawing requirement.

Frequently Asked Questions

Q: What is the yield strength of GH5188 bar?

A: In the cold worked and aged condition the yield strength is approximately 690 MPa to 1035 MPa, depending on the amount of cold work, the aging treatment and the composition of the heat.

Q: What tensile strength can be expected?

A: The tensile strength is generally above 1200 MPa in the high strength condition.

Q: Why is the elongation relatively low?

A: The high strength condition is obtained by cold work and aging, which raises strength at the expense of ductility, so elongation is typically below 15 percent.

Q: What is the typical hardness range?

A: Approximately 30 to 40 HRC in the cold worked and aged condition.

Q: How are the properties verified?

A: By tensile testing in accordance with GB/T 228.1 and by hardness measurement on the finished bar, with the results recorded on the certificate.

Q: Does heat treatment affect the property level?

A: Yes. The solution treated condition gives lower strength and higher ductility, while cold work followed by aging gives the high strength condition, so the condition must always be specified with the property values.