LR EH42 is an extra-high-strength marine steel plate certified by Lloyd's Register (LR). The "EH" designation signifies it is impact tested at -40°C, ensuring excellent toughness for vessels operating in cold environments . It has a minimum yield strength of 420 MPa and tensile strength ranging from 530 to 680 MPa, with minimum elongation of 20% . Its chemical composition is strictly controlled with carbon ≤0.20% and manganese ≤1.70% .
LR EH50 is an ultra-high-strength marine steel plate also certified by Lloyd's Register (LR), with impact toughness tested at -40°C . The "50" denotes a minimum yield strength of 500 MPa and tensile strength ranging from 610 to 770 MPa, with minimum elongation of 18% . Impact energy requirements are 33J (transverse) or 50J (longitudinal) at -40°C . This grade is designed for demanding structural components requiring superior strength-to-weight ratio.
Both LR EH42 and LR EH50 are LR-certified extra-high-strength marine steels with excellent low-temperature toughness tested at -40°C, ensuring reliable performance in harsh marine environments . Their primary difference lies in strength level: EH42 offers a minimum yield strength of 420 MPa with tensile strength of 530-680 MPa, suitable for high-strength hull construction, while EH50 provides a substantially higher minimum yield strength of 500 MPa with tensile strength reaching 610-770 MPa, designed for more demanding load-bearing applications requiring superior strength-to-weight ratio . Both grades feature controlled chemical composition (carbon ≤0.20%, manganese ≤1.70%) and maintain good weldability for critical marine service.
Chemical Composition
|
LR EH42 extra high Strength Chemical Composition |
|||||||
|
Grade |
The Element Max (%) |
||||||
|
C |
Si |
Mn |
P |
S |
Al |
N |
|
|
LR EH42 |
0.20 |
0.55 |
1.70 |
0.030 |
0.030 |
0.015 |
0.020 |
|
Nb |
V |
Ti |
Cu |
Cr |
Ni |
Mo |
|
|
0.02-0.05 |
0.03-0.10 |
0.02 |
|
|
|
|
|
|
LR EH50 extra high Strength Chemical Composition |
|||||||
|
Grade |
The Element Max (%) |
||||||
|
C |
Si |
Mn |
P |
S |
Al |
N |
|
|
LR EH50 |
0.20 |
0.55 |
1.70 |
0.030 |
0.030 |
0.015 |
0.020 |
|
Nb |
V |
Ti |
Cu |
Cr |
Ni |
Mo |
|
|
0.02-0.05 |
0.03-0.10 |
0.02 |
|
|
|
|
|
Mechanical Property
|
LR EH42 extra high strength property |
|||||||
|
Grade |
|
Mechanical Property |
Charpy V Impact Test |
||||
|
Thickness |
Yield |
Tensile |
Elongation |
Degree |
Energy 1 |
Energy 2 |
|
|
LR EH42 |
mm |
Min Mpa |
Mpa |
Min % |
-40 |
J |
J |
|
t≤50 |
420 |
530-680 |
20% |
28 |
42 |
||
|
50<t≤70 |
420 |
530-680 |
20% |
28 |
42 |
||
|
70<t≤100 |
420 |
530-680 |
20% |
28 |
42 |
||
|
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
|||||||
|
LR EH50 extra high strength property |
|||||||
|
Grade |
|
Mechanical Property |
Charpy V Impact Test |
||||
|
Thickness |
Yield |
Tensile |
Elongation |
Degree |
Energy 1 |
Energy 2 |
|
|
LR EH50 |
mm |
Min Mpa |
Mpa |
Min % |
-40 |
J |
J |
|
t≤50 |
500 |
610-770 |
18% |
33 |
50 |
||
|
50<t≤70 |
500 |
610-770 |
18% |
33 |
50 |
||
|
70<t≤100 |
500 |
610-770 |
18% |
33 |
50 |
||
|
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
|||||||