SN490C belongs to the JIS G3136 family of rolled steels for building structures, the SN series that also includes SN400B, SN400C, SN490B and the lower strength SN400 grades. The series was introduced to give steel building frames predictable plastic deformation capacity, because ordinary structural plate of the same strength level does not guarantee the combination of narrow yield range, limited yield ratio and toughness that seismic design assumes.
Grade Position Within JIS G3136
| Designation | Tensile class | Impact test temperature | Typical use |
|---|---|---|---|
| SN400B | 400 MPa class | 0 C | Beams and secondary members |
| SN400C | 400 MPa class | 0 C, tightened P and S | Seismic frames, welded box sections |
| SN490B | 490 MPa class | 0 C | Columns and heavy frames |
| SN490C | 490 MPa class | 0 C, tightened P and S | Heavily welded columns and nodes |
The final letter is the key differentiator inside the series: the C grades apply tighter limits on phosphorus and sulphur, plus carbon equivalent and weld crack sensitivity controls, which is why they are specified for heavily welded connections where the B grade would be marginal.
Chemical Composition of SN490C
| Element | Requirement | Effect on fabrication |
|---|---|---|
| C | 0.18 % max | Caps hardness and cracking risk in the heat-affected zone |
| Si | 0.55 % max | Deoxidation control without impairing toughness |
| Mn | 1.60 % max | Provides strength while retaining ductility |
| P | 0.020 % max | Reduces segregation and temper embrittlement risk |
| S | 0.008 % max | Minimises lamellar tearing and inclusion-related defects |
Phosphorus at 0.020 % and sulphur at 0.008 % are the fingerprints of a C grade. Together with a restricted carbon content they keep carbon equivalent, normally expressed to the IIW formula, inside the range that building codes accept for thick welded joints without exceptional preheat. The C grade is also assessed for weld crack sensitivity, so the composition balance rather than carbon alone governs acceptance.
Mechanical Properties and Ductility Requirements
| Property | Requirement for SN490C |
|---|---|
| Yield strength | 325 MPa minimum |
| Tensile strength | 490-610 MPa |
| Elongation | 17 % minimum for the standard plate thickness range |
| Charpy V-notch absorbed energy | 27 J minimum at 0 C |
| Yield ratio | 0.80 maximum |
| Yield strength variation | Within 120 MPa across the supplied range |
The last two items are what separate SN490C from a plain 490 MPa structural steel. A yield ratio capped at 0.80 guarantees a plastic plateau before strain hardening, and holding the yield strength variation inside 120 MPa stops an unexpectedly strong plate from pulling load into a connection that was designed for a lower value. Both properties matter more in a moment frame than the nominal strength itself.
Through-Thickness and Dimensional Behaviour
Thickness direction ductility is controlled: the reduction of area in a through-thickness tensile test is required to be 25 % or greater, which limits lamellar tearing in welded T-joints and corner joints.
Dimensional tolerances are tightened relative to general structural plate, so a fabricated frame does not have to absorb the wider minus tolerances common in commodity plate.
Plate supplied to the C grade is intended for welded box columns, beam-to-column connections and other details where restraint is high in all three directions.
These requirements are the practical reason a fabricator pays a premium for SN490C instead of ordering a general 490 MPa plate and adding extra inspection. The properties are built into the product rather than proven afterwards on a case by case basis.
Fabrication and Welding Practice
SN490C welds like a low-carbon, micro-alloyed structural steel but with a narrower process window than ordinary plate. The tightening that matters most in the shop is sulphur control, which reduces the risk of lamellar tearing in thick restrained joints, and carbon equivalent control, which keeps required preheat at moderate levels. Typical shop practice for building work includes the following points.
Filler metals should match the 490 MPa tensile class, and low-hydrogen consumables are used for thick or restrained joints.
Heat input should be recorded rather than assumed, because the same grade is used from 6 mm plate up to heavy sections and no single setting is correct across that range.
Welding procedures and welders are qualified to the requirements of the project, and building steel work in Japan is additionally executed under the architectural steel work specification JASS 6.
Ultrasonic testing is normally applied to full penetration connections in seismic frames, since the design depends on weld soundness rather than on overstrength of the base metal.
Common thickness ranges for SN490C run from thin plate used in built-up sections up to heavy plate for column bases and nodes, and the grade is normally supplied in the as-rolled or controlled-rolled condition. Normalising, quenching and tempering are not part of the standard delivery condition for this grade, and heat treatment beyond what the specification requires should not be assumed by the fabricator.
Applications
SN490C is used for columns, transfer beams and moment connections in multi-storey building frames, for large-span roof structures, and for equipment support frames where seismic ductility is required. Because its yield ratio and toughness are guaranteed, it is preferred over general structural plate wherever a connection has to yield in a controlled way before it fractures. Designers working to Japanese practice pair it with the building standard requirements for structural steel, while international projects frequently specify it by equivalent property requirements in their own design codes.
Frequently Asked Questions
Q: What is SN490C steel plate?
It is a rolled steel for building structures defined by JIS G3136, with a 490 MPa class tensile strength of 490-610 MPa, a minimum yield strength of 325 MPa, and additional controls on yield ratio, carbon equivalent and through-thickness ductility.
Q: How does SN490C differ from SN490B?
The C grade applies tighter phosphorus and sulphur limits, at 0.020 % and 0.008 %, together with weld crack sensitivity controls. Those tighter limits make it better suited to heavily welded, highly restrained connections.
Q: Why is the yield ratio limited to 0.80?
A capped yield ratio ensures the steel deforms plastically before it strain hardens, so a frame can absorb seismic energy through controlled yielding. It is one of the defining ductility requirements of the SN series.
Q: Why must the yield strength variation stay within 120 MPa?
Large variation would concentrate deformation in the weaker plate of a connection and overload the stronger one, so JIS G3136 restricts the spread to keep the designed load path predictable.
Q: What does the 25 % through-thickness reduction of area requirement achieve?
It limits lamellar tearing, which occurs when sulphur inclusions in a thick restrained joint separate under through-thickness strain. A guaranteed reduction of area gives the fabricator confidence in T-joints and corner joints.
Q: Is SN490C supplied quenched and tempered?
No. SN490C is normally supplied as rolled or controlled rolled. Quenched and tempered behaviour belongs to high-strength grades such as S690QL to EN 10025-6, which is a different product family.