What Is Q620 Steel Plate?
Q620 is a Chinese designation for a high-strength structural steel plate with a guaranteed minimum yield strength of 620 MPa. Under GB/T 16270-2009, the standard for high strength structural steel plates in the quenched and tempered condition, Q620 plate is supplied in the quenched and tempered (Q+T) state in thicknesses up to 150 mm. The letter Q stands for yield strength, 620 is the minimum yield value in MPa, and the suffix letter C, D, E or F is the quality grade, which fixes the impact test temperature.
Q620 belongs to the low-alloy high-strength family often labelled HSLA. Carbon is kept low and the strength comes from a quench-and-temper treatment combined with small additions of microalloying elements. Because the guaranteed yield is about 75 % higher than that of an ordinary structural steel such as Q355 at 355 MPa, a designer can reduce section thickness, which lowers both steel tonnage and fabricated weight.
A note on standards: Q620 also appears in GB/T 1591, the general low-alloy high-strength structural steel standard, where the property brackets are different - the 620 MPa yield guarantee applies only up to 16 mm thickness. The governing standard should therefore be stated on the order, because the mechanical guarantees of the two standards are not interchangeable.
Chemical Composition and Mechanical Properties
Maximum heat-analysis values per GB/T 16270-2009, weight per cent.
| Element | Max % | Element | Max % |
|---|---|---|---|
| C | 0.20 | Si | 0.80 |
| Mn | 1.70 | P | 0.020 |
| S | 0.010 | Cu | 0.50 |
| Cr | 1.50 | Ni | 2.00 |
| Mo | 0.70 | B | 0.0050 |
| V | 0.12 | Nb | 0.06 |
| Ti | 0.05 |
The tight sulphur limit of 0.010 % and the low phosphorus limit of 0.020 % are typical of a quenched and tempered plate, because cleanliness supports the toughness that the grade promises at low temperature. Chromium, nickel, molybdenum and boron are the alloying elements that allow the plate to harden through the section during quenching and then temper back to a strong, tough structure without an excessive carbon content.
| Thickness T (mm) | Yield ReH min (MPa) | Tensile Rm (MPa) | Elongation A min (%) |
|---|---|---|---|
| T ≤ 50 | 620 | 700-890 | 15 |
| 50 < T ≤ 100 | 580 | 700-890 | 15 |
| 100 < T ≤ 150 | 560 | 650-830 | 15 |
Values are per GB/T 16270-2009. Tensile tests use transverse specimens and impact tests use longitudinal Charpy V-notch specimens. Where the stress-strain curve shows no distinct yield point, the Rp0.2 proof strength is reported instead of ReH. Note that the yield guarantee steps down above 50 mm and again above 100 mm, so the design stress has to be checked against the bracket that is actually ordered.
Quality Grades Q620C, Q620D, Q620E and Q620F
The suffix letter determines the impact test temperature, not the strength. The grade should be chosen from the lowest service temperature of the component.
| Grade | Impact test temp | KV2 min, longitudinal | Typical selection |
|---|---|---|---|
| Q620C | 0 °C | 47 J | Indoor or warm-climate structures |
| Q620D | -20 °C | 47 J | General outdoor structures |
| Q620E | -40 °C | 47 J | Cold regions, mining machinery, port equipment |
| Q620F | -60 °C | 47 J | Arctic service and extreme low-temperature projects |
Impact energy is the mean of three specimens; a single specimen may fall below the required mean but not below 70 % of it. Reduced-size specimens are used for 6-12 mm plate, as the standard provides. Where lamellar tearing resistance matters in heavy welded joints, Z-direction properties at Z15, Z25 or Z35 can be specified for plate 15 mm and thicker, tested to GB/T 5313.
Q620 Compared with Q550 and Q690
The three grades form a strength ladder inside the same standard; values below are per GB/T 16270-2009 for thickness up to 50 mm.
| Grade | Min yield (t ≤ 50 mm) | Tensile Rm (MPa) | Elongation A |
|---|---|---|---|
| Q550 | 550 MPa | 640-820 | ≥ 16 % |
| Q620 | 620 MPa | 700-890 | ≥ 15 % |
| Q690 | 690 MPa | 770-940 | ≥ 14 % |
Moving from Q550 to Q620 raises the guaranteed yield by about 13 %, and from Q620 to Q690 by about 11 %, while the elongation allowance and the carbon equivalent control tighten in parallel. In practice the choice follows design stress and fabrication cost: Q620 sits at a common middle point where plate can still be welded with controlled procedures and heavy sections stay within the 150 mm limit of the quenched and tempered standard.
Welding, Fabrication and Applications
Q620 obtains its strength from the quench-and-temper treatment, and welding reheats the heat-affected zone locally, so the joint has to be protected by procedure rather than by the base plate alone. Work to a qualified welding procedure specification and apply these rules of thumb:
Preheat: typically 100-180 °C, set from thickness and carbon equivalent; plate of 50 mm and above usually starts at 120-180 °C.
Consumables: low-hydrogen types matched to the 620 MPa tensile level, such as the E9018-G classification; store and dry them as recommended by the manufacturer.
Heat input: keep it low and controlled - multi-pass rather than single large passes - and limit interpass temperature, typically to 220 °C or below, to protect heat-affected-zone toughness.
Hydrogen control: clean and dry the joint faces and remove moisture, oil and scale before welding.
Post-weld heat treatment: normally not required; where the design calls for stress relief at around 580-620 °C for very thick or highly restrained joints, confirm it against the procedure and the plate certificate.
For critical structures, pre-production weld tests are run and, where the project requires it, independent inspection of the completed joints is arranged. Typical applications include mining machinery such as dump-truck bodies, excavator booms and hydraulic support beams; cranes and lifting equipment such as telescopic booms, chassis frames and slewing rings; bridges and steel structures such as main girders, heavy columns and truss nodes; pressure vessel supports, skirts, brackets and structural frames; port and offshore equipment such as gantry cranes, ship unloaders and platform supports; and heavy transport equipment such as low-bed trailers and transporter frames.
Frequently Asked Questions About Q620 Steel Plate
Q: Which standard governs Q620 steel plate?
GB/T 16270-2009 for high strength structural steel plates in the quenched and tempered condition, which covers thickness up to 150 mm. Q620 also appears in GB/T 1591 with different property brackets, so the governing standard should be stated on the order.
Q: What is the minimum yield strength of Q620?
620 MPa for thickness up to 50 mm, 580 MPa from 50 to 100 mm and 560 MPa from 100 to 150 mm, with a tensile strength of 700-890 MPa for the thinner two brackets and 650-830 MPa above 100 mm.
Q: How do I choose between the C, D, E and F grades?
By impact test temperature: 0 °C, -20 °C, -40 °C and -60 °C respectively, each with a minimum longitudinal Charpy energy of 47 J. Pick the grade from the lowest service temperature of the component.
Q: Is Q620 weldable?
Yes, with a qualified procedure. Quenching and tempering raises the carbon equivalent compared with lower-strength grades, so preheat of roughly 100-180 °C, low-hydrogen consumables and a limited interpass temperature are used to protect the heat-affected zone.
Q: Does Q620 need post-weld heat treatment?
Normally not. Stress relief at around 580-620 °C is applied only where the design requires it for very thick or highly restrained joints, and it should be confirmed against the welding procedure and the plate certificate.
Q: Can Z-direction properties and ultrasonic testing be added?
Yes. Through-thickness properties at Z15, Z25 or Z35 can be specified for plate 15 mm and thicker, tested to GB/T 5313, and ultrasonic testing can be specified to GB/T 2970 together with an EN 10204 3.1 mill test certificate.