EN10028-3 P275NL1 is a pressure vessel steel grade that is widely used in the fabrication of pressure vessels and boilers due to its excellent mechanical properties and chemical composition. This grade is designed to operate at low temperatures, making it suitable for applications in the petrochemical, chemical, and energy industries where low-temperature resistance is a critical requirement.
Chemical Composition:
The chemical composition of EN10028-3 P275NL1 is carefully controlled to ensure the material's toughness and weldability. The typical chemical composition includes:
|
P275NL1 Chemical Composition |
|||||||
|
Grade |
The Element Max (%) |
||||||
|
C |
Si |
Mn |
P |
S |
Al(min) |
N |
|
|
P275NL1 |
0.16 |
0.40 |
0.5-1.40 |
0.030 |
0.020 |
|
0.02 |
|
Cr |
Cu |
Mo |
Nb |
Ni |
Ti |
V |
|
|
0.30 |
0.30 |
0.08 |
0.005 |
0.50 |
0.03 |
0.05 |
|
Carbon Equivalent: Ceq = 【C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15】%
Mechanical Properties:
The mechanical properties of P275NL1 are characterized by its high strength and good ductility, which are essential for pressure vessel applications. The typical mechanical properties are as follows:
|
Grade |
|
P275NL1 Mechanical Property |
|||||
|
Thickness |
Yield |
Tensilmie |
Elongation |
Impact Energy(KV J) min |
|||
|
P275NL1 |
mm |
Min Mpa |
Mpa |
Min % |
-20° |
0° |
+20° |
|
≤ 16 |
275 |
390-510 |
24 |
47 |
55 |
63 |
|
|
16> to ≤35 |
275 |
390-510 |
24 |
47 |
55 |
63 |
|
|
35> to ≤50 |
265 |
390-510 |
24 |
47 |
55 |
63 |
|
|
50> to ≤70 |
255 |
390-510 |
24 |
47 |
55 |
63 |
|
|
70> to ≤100 |
235 |
370-490 |
23 |
47 |
55 |
63 |
|
|
100> to ≤150 |
235 |
350-470 |
23 |
47 |
55 |
63 |
|
Heat Treatment:
P275NL1 is generally supplied in the normalized condition. Normalization is a heat treatment process that refines the grain structure and improves the mechanical properties of the steel. The steel is heated to a temperature above its upper critical point and then cooled in air.
Low-Temperature Impact Test:
The material is subjected to a low-temperature impact test to ensure its toughness at sub-zero temperatures. The impact energy values are measured at -40°C, which is a standard temperature for low-temperature applications.
|
Equivalent steel grade of P275NL1 |
|||||||
|
Europe |
Belgium |
Germany |
BS 1501 |
Italy |
ASTM |
India |
Japan |
|
|
|
TSt E285 |
|
|
A662 Gr. A |
|
|