What Is LR EH62 Shipbuilding Steel Plate?
LR EH62 is an extra high strength shipbuilding steel plate produced in the Lloyd's Register grade series for shipbuilding and ocean offshore structural projects. The designation carries three pieces of information: the letter E means the steel is Charpy V-notch impact tested at -40 °C, the letter H identifies a higher strength hull structural steel rather than a normal strength grade, and 62 states a minimum yield strength of 620 MPa. Engineers specify this grade when a structural detail needs very high strength together with reliable low temperature toughness and predictable welding behaviour.
Because EH62 sits at the top of the extra high strength range, plates are normally supplied quenched and tempered or thermo-mechanically controlled processed. Carbon, sulphur, phosphorus and nitrogen are held at low levels so that the carbon equivalent stays inside a window that shipyards can weld with qualified procedures, and so that heat affected zone toughness does not fall below the class requirement.
Chemical Composition of LR Grade EH62
The table below lists typical maximum values for the ladle analysis of EH62 plate. Niobium, vanadium and titanium are used in combination as micro-alloying additions to control grain size, which is the main lever for reaching -40 °C impact energy in a steel with 620 MPa minimum yield strength.
| Element | Typical value (%) |
|---|---|
| C | 0.20 max |
| Si | 0.55 max |
| Mn | 1.70 max |
| P | 0.030 max |
| S | 0.030 max |
| Al | 0.015 min |
| N | 0.020 max |
| Nb | 0.02 - 0.05 |
| V | 0.03 - 0.10 |
| Ti | 0.02 max |
| Cu | 0.35 max |
| Cr | 0.20 max |
| Ni | 0.40 max |
| Mo | 0.08 max |
Copper, chromium, nickel and molybdenum are residual and control elements rather than deliberate alloy additions at these levels; the maximum permissible values come from the class rules, and the mill certificate issued with every heat records the actual analysis of the delivered plate.
Mechanical Properties and Impact Energy
Minimum mechanical requirements are held constant across the full thickness range covered by the grade, which simplifies the design of heavy structural sections and keeps one material certificate valid for a wide spread of plate sizes.
| Thickness (mm) | Yield strength min (MPa) | Tensile strength (MPa) | Elongation min (%) | Charpy V at -40 °C, transverse (J) | Charpy V at -40 °C, longitudinal (J) |
|---|---|---|---|---|---|
| t ≤ 50 | 620 | 720 - 890 | 17 | 41 | 62 |
| 50 < t ≤ 70 | 620 | 720 - 890 | 17 | 41 | 62 |
| 70 < t ≤ 100 | 620 | 720 - 890 | 17 | 41 | 62 |
Tensile testing is normally performed on specimens taken transverse to the final rolling direction, and three impact specimens are tested for each condition. The longitudinal energy requirement is higher than the transverse requirement because rolled plate is tougher along the rolling direction; designers therefore state the specimen orientation that matches the controlling stress direction in the joint.
Delivery Condition, Testing and Certification
EH62 plate is ordered in one or more of the following delivery conditions, depending on the design code and the fabrication route of the yard:
As rolled, for thinner sections where the rolling schedule alone develops the required properties
Normalized or normalized and tempered
Thermo-mechanically controlled processed
Quenched and tempered
Supplementary requirements frequently ordered with this grade include ultrasonic examination of the full plate area, through thickness property testing in the Z15, Z25 or Z35 direction for tee joints and restrained connections, additional impact testing at lower temperatures, independent third party inspection witnessed by a surveyor, and surface preparation by shot blasting and priming for protection during transport and storage.
Applications and Fabrication Notes
EH62 plate is selected for structural locations where the weight saving achieved by a 620 MPa yield steel justifies the higher material and fabrication cost:
Primary hull structures of large commercial vessels, including sheer strake and strength deck areas
Offshore platforms, jack-up legs and ocean offshore structural projects
Ice class hull regions where low temperature toughness is mandatory
Heavy lift vessels, cranes and deck equipment foundations
Drilling ships, floating production units and conversion projects
Fabrication of this grade requires three controls. Welding procedures must be qualified with heat affected zone toughness testing at -40 °C matching the base plate requirement; preheat and interpass temperatures must follow the carbon equivalent and thickness of the joint; and cutting must avoid local hardening. Plates are cut by flame, plasma, laser or abrasive water jet depending on thickness, and heavy sections are preheated before flame cutting so that the cut edge does not crack during handling. Bending and forming are carried out warm or with generous bend radii, because the high yield strength of the grade limits cold forming capacity compared with normal strength hull steels.
FAQ about LR EH62 Steel Plate
Q: What does the EH62 designation mean?
E means Charpy V-notch impact testing at -40 °C, H identifies a higher strength hull structural steel, and 62 is the minimum yield strength in MPa.
Q: What is the minimum yield strength of LR EH62?
620 MPa across the standard thickness range, with tensile strength between 720 and 890 MPa and minimum elongation of 17 %.
Q: How does EH62 differ from EH40?
EH40 requires 390 MPa minimum yield strength while EH62 requires 620 MPa, so EH62 needs a richer alloy design and more tightly controlled rolling and heat treatment.
Q: Which thickness range is available?
Plates are commonly rolled from 8 mm up to about 100 mm in this grade, with additional thickness options depending on the approved rolling route and heat treatment capacity of the mill.
Q: What impact energy is required at -40 °C?
41 J minimum in the transverse direction and 62 J minimum in the longitudinal direction, measured on Charpy V-notch specimens.
Q: Can LR EH62 be welded in a shipyard?
Yes. Welding procedures must be qualified to the class rules, preheat and interpass temperature must be controlled, and consumables must match the strength and toughness of the base plate.