ABS FQ47 is an extra-high-strength marine steel plate certified by the American Bureau of Shipping (ABS) . The "FQ" designation signifies it is a quenched and tempered steel with impact toughness tested at -60°C , ensuring exceptional performance in polar and Arctic environments . It has a minimum yield strength of 460 MPa and a tensile strength ranging from 570 to 720 MPa , with a minimum elongation of 17% . This grade is widely used in offshore drilling platforms, ship hulls, and critical marine structures requiring high strength and excellent corrosion resistance .
ABS FQ70 is an ultra-high-strength marine steel plate also certified by ABS, manufactured through quenching and tempering processes . Like FQ47, it is impact tested at -60°C , with minimum impact energy requirements of 46J (transverse) and 69J (longitudinal) . The "70" denotes a minimum yield strength of 690 MPa and a tensile strength ranging from 770 to 940 MPa , with a minimum elongation of 14% . Its chemical composition is strictly controlled with carbon ≤0.18% and manganese ≤1.60% . This grade is designed for the most demanding applications, including jack-up rig legs, ultra-large container vessels, and critical marine structures requiring maximum strength-to-weight ratio .
Both ABS FQ47 and ABS FQ70 are ABS-certified quenched and tempered marine steels with exceptional low-temperature toughness tested at -60°C , ensuring reliable performance in the most extreme Arctic and harsh marine environments . Their primary difference lies in strength level: FQ47 offers a minimum yield strength of 460 MPa with tensile strength of 570-720 MPa, suitable for high-strength offshore platforms and ship hulls , while FQ70 provides a substantially higher minimum yield strength of 690 MPa with tensile strength reaching 770-940 MPa, designed for the most demanding load-bearing applications requiring maximum weight reduction . Both grades feature strictly controlled chemical composition (carbon ≤0.18%) and maintain good weldability for critical marine service.
Chemical Composition
|
ABS FQ47 Extra high Strength Chemical Composition in Tempering and Quenching |
||||||
|
Grade |
The Element Max (%) |
|||||
|
C |
Si |
Mn |
P |
S |
N |
|
|
ABS FQ47 |
0.18 |
0.55 |
1.60 |
0.025 |
0.025 |
0.02 |
|
ABS FQ70 Extra high Strength Chemical Composition in Tempering and Quenching |
||||||
|
Grade |
The Element Max (%) |
|||||
|
C |
Si |
Mn |
P |
S |
N |
|
|
ABS FQ70 |
0.18 |
0.55 |
1.60 |
0.025 |
0.025 |
0.02 |
Mechanical Property
|
ABS FQ47 Extra high strength property in tempering and quenching |
||||||
|
Grade |
Mechanical Property |
Charpy V Impact Test |
||||
|
Yield |
Tensile |
Elongation |
Degree |
Energy 1 |
Energy 2 |
|
|
Min Mpa |
Mpa |
Min % |
-40 |
J |
J |
|
|
ABS FQ47 |
460 |
570-720 |
17 |
31 |
46 |
|
|
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
||||||
|
ABS FQ70 Extra high strength property in tempering and quenching |
||||||
|
Grade |
Mechanical Property |
Charpy V Impact Test |
||||
|
Yield |
Tensile |
Elongation |
Degree |
Energy 1 |
Energy 2 |
|
|
Min Mpa |
Mpa |
Min % |
-60 |
J |
J |
|
|
ABS FQ70 |
690 |
770-940 |
14 |
41 |
62 |
|
|
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
||||||