ASTM A537 Class 3 Steel Plate: Chemical Composition and Mechanical Properties

Sep 25, 2025 Leave a message

ASTM-A537-A537M-Standard-Specification.pdf

ASTM A537 Class 3 Steel Plate Overview

ASTM A537 Class 3 is a quenched and tempered carbon-manganese-silicon steel plate produced under ASTM A537/A537M for fusion welded pressure vessels, boilers, storage tanks and structural pressure parts. The grade is supplied in three classes that differ in heat treatment, and Class 3 is the quenched and tempered class, chosen when a higher strength level must be combined with good notch toughness in thick sections.

The alloy design is deliberately simple: carbon, manganese and silicon provide the strength and hardenability, while tight control of phosphorus and sulfur keeps the steel clean and weldable. Because the chemistry is lean, A537 Class 3 plate remains economical compared with low alloy pressure vessel steels while still satisfying the design stresses used in large welded vessels and tanks.

Chemical Composition of A537 Class 3

The table below lists the element limits for the class. Values shown are maximums unless a range is given. Carbon equivalent is calculated with the standard formula Ceq = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15 and is normally reported on the mill certificate so that the fabricator can set welding parameters.

Element Limit (%)
C, max 0.24
Mn 0.92-1.72
P, max 0.035
S, max 0.035
Si 0.13-0.55
Cu, max 0.38
Ni, max 0.28
Cr, max 0.29
Mo, max 0.09

The manganese range of 0.92-1.72% is wide because the class is produced in a broad thickness range and the mill adjusts manganese with section size to hold the required strength through the thickness. Residual elements such as copper, nickel, chromium and molybdenum are capped so that the carbon equivalent stays predictable and welding procedures qualified on one heat remain valid for the next.

Mechanical Properties by Thickness

Yield strength and tensile strength requirements fall as plate thickness increases, because heavier sections cool more slowly during quenching and develop a coarser microstructure. The tabulated requirements for the class are summarised below.

Thickness range (mm) Yield strength, min (MPa) Tensile strength (MPa) Elongation, min (%)
6-65 380 550-690 22
65-100 345 515-655 20
100-150 275 485-620 Reported

Tension tests are taken in the direction required by the specification and the elongation values apply to the gauge length stated for the class. Impact testing is performed on Charpy V-notch specimens when the order requires it, and the test temperature is agreed from the minimum design metal temperature of the vessel.

Dimensions, Heat Treatment and Additional Conditions

A537 Class 3 plate is rolled from 6 mm to 300 mm in thickness, with width normally between 1500 mm and 4200 mm and length between 3000 mm and 18000 mm. Thickness, width, length and flatness tolerances are taken from ASTM A6. Quenching is carried out in a continuous roller pressure quench or a tank quench, and tempering follows immediately so that the plate leaves the line with a stable, uniform structure.

Rolling type: boiler and pressure vessel quality plate.

Heat treatment: quenched and tempered; normalized or thermo-mechanically controlled processing is available for other classes and agreements.

Ultrasonic examination: available for the full plate body or for edge zones.

Z direction testing: Z15, Z25 and Z35 through-thickness tensile testing on request.

Charpy V-notch impact testing: performed at the temperature specified for the duty.

Surface treatment: shot blasting, priming and painting can be applied at the mill.

Certification: material test certificates to EN 10204 type 3.1 with full traceability.

Fabrication Notes for Pressure Vessel Shops

The class is designed for fusion welding, and its moderate carbon equivalent allows shielded metal arc, submerged arc, gas metal arc and flux cored welding without special measures beyond those required by the vessel code. Preheat is normally applied as a function of thickness and hydrogen level of the consumable, and post-weld heat treatment is applied where the design code requires stress relief. Cold forming of heads and shells is carried out before the final heat treatment when the forming strain is high, so that the quenching and tempering cycle covers the cold worked material.

FAQ

Q: What is ASTM A537 Class 3 plate used for?
It is used for fusion welded pressure vessels, boilers, steam drums, storage tanks, heat exchangers and large structural pressure parts where higher strength and reliable toughness are both needed.

Q: How does Class 3 differ from the other classes?
The classes share the same chemistry but differ in heat treatment and in the resulting property levels. Class 3 is the quenched and tempered class, so the class must always be quoted together with the grade on an enquiry.

Q: What thickness is available?
Plate is normally rolled from 6 mm to 300 mm. Mechanical property requirements are tabulated by thickness band, so heavier plate is ordered against the corresponding band for the design calculation.

Q: Is A537 Class 3 impact tested?
Charpy V-notch testing is specified for the class, and the test temperature is selected from the minimum design metal temperature of the equipment. Test results are reported on the mill certificate.

Q: Can through-thickness properties be guaranteed?
Yes. Z15, Z25 and Z35 through-thickness tensile testing can be arranged when the joint design creates a risk of lamellar tearing, and the results are certified with the plates.

Q: Why is carbon equivalent reported?