A 537 Class 2 steel plates

Sep 25, 2025 Leave a message

ASTM-A537-A537M-Standard-Specification.pdf

The ASTM A537 specification is the Standard Specification for Pressure Vessel Plates, Heat-Treated, Carbon-Manganese-Silicon Steel used in the applications of fusion welded pressure vessels and structures. Typical applications are pressure vessels designed for moderate and lower-temperature service requiring excellent notch toughness as well as API 650 and API 620 storage tanks. Class 1 material is available as Normalized and Class 2 is available as Quenched & Tempered plates.

 

Dimension Range

Thickness
(in)

Width
(in)

Length
(in)

0.375 - 2.00

96 - 120

240 - 588

 

 

Mechanical Properties

Tensile testing is performed in the transverse direction according to ASTM A20 requirements. The required mechanical properties are tabulated below:

Grade

Yield strength
(min ksi)

Tensile strength
(ksi)

Elongation in 2"
(min %)

A537 Class 2

60

80 - 100

22

Mechanical testing

Charpy V-Notch Impact Toughness requirements may be ordered as a supplementary requirement (S5). A minimum Charpy V-notch impact energy value of 30 ft-lbs [41 J] at - 40°F [-40°C] in longitudinal specimens is a typical supplemental impact toughness requirement. Please inquire for applications requiring a specified minimum impact toughness.

 

Chemical Composition

C
(max wt %)

Mn 1)
(max wt %)

P 2)
(max wt %)

S 2)
(max wt %)

Si
(max wt %)

Cu
(max wt %)

Ni 1)
(max wt %)

Cr
(max wt %)

Mo
(max wt %)

0.24

1.60

0.020

0.010

0.50

0.35

0.25

0.25

0.080

1) Manganese may exceed 1.35 % on heat analysis, up to a maximum of 1.60 %, and nickel may exceed 0.25 % on heat analysis, up to a maximum of 0.50 %, provided the heat analysis carbon equivalent (CEV) does not exceed 0.57 %.

2) P and S are more restrictive than A537/SA537 requirements. Even lower limits for P and S are available on an inquiry basis.

 

Carbon Equivalent

Thickness (in)

0.375 - 2.00

Typical CET (wt %)

0.33

Typical CEV (wt %)

0.45