ASTM A515 Gr 70 Plate for Boilers and Pressure Tanks

Nov 18, 2025 Leave a message

What ASTM A515 Gr 70 Plate Is

ASTM A515 Gr 70 is a carbon-silicon steel plate made to ASTM A515 / ASME SA515 for intermediate- and higher-temperature service in welded boilers and pressure vessels. The grade number refers to a minimum tensile strength of 70 ksi, approximately 485 MPa. Plates are normally supplied in the normalized condition, which refines the grain structure and gives a useful balance of strength, ductility and toughness for stationary equipment such as boiler drums, shells, heads and storage tanks.

Because A515 Gr 70 is a plain carbon-silicon grade rather than a low-alloy steel, it remains one of the most economical materials able to carry hot, pressurized loads. Its weldability and predictable behaviour during fabrication are the reasons it stays a first choice for power generation, petrochemical and general heavy-industry equipment.

Chemical Composition and Mechanical Properties

Silicon is deliberately added as a deoxidizing and strengthening element, which is the main metallurgical difference between the A515 family and the silicon-killed A516 plate used at lower service temperatures. Typical limits are summarised below.

Element Typical limit, %
Carbon (C) 0.31 max, ladle
Manganese (Mn) 1.20 max
Silicon (Si) 0.13 - 0.45
Phosphorus (P) 0.035 max
Sulfur (S) 0.035 max

Exact limits depend on plate thickness and on the edition of ASTM A515 / ASME SA515 named in the purchase order, so the mill certificate should always be checked against the ordered specification before fabrication starts.

Property Value
Minimum yield strength 260 MPa (38 ksi)
Tensile strength 485 - 620 MPa (70 - 90 ksi)
Minimum elongation, 200 mm gauge 17 %
Minimum elongation, 50 mm gauge 21 %
Typical hardness Under 200 HB
Density 7.80 g/cm3

Supply Condition, Heat Treatment and Dimensions

Supply condition: as-rolled, normalized, normalized and tempered, or quenched and tempered, with normalizing the usual choice for boiler and pressure vessel work.

Thickness: commonly 6 mm to 300 mm, depending on mill capability.

Width: 1500 mm to 4050 mm; length: 3000 mm to 15000 mm.

Finish: hot rolled plain plate; surface quality follows the plate specification rather than a decorative standard.

Documentation: mill test certificates to EN 10204 3.1 or 3.2, with third-party inspection when required.

Stress relieving after cold forming or welding is decided by the applicable construction code and by plate thickness. Where the code requires it, the treatment is carried out below the lower critical temperature so that the normalized microstructure is not destroyed.

Fabrication and Welding Behaviour

A515 Gr 70 welds well with the usual arc processes: shielded metal arc welding, submerged arc welding and gas metal arc welding are all used in boiler shop practice. Preheating requirements are modest, typically in the 80 - 120 degree C range for heavy sections, and are set mainly by thickness and by the restraint of the joint. Because the steel is a carbon-silicon grade with a moderate carbon level, it does not demand the careful low-hydrogen regime of a quenched and tempered low-alloy plate, but consumables should still match the strength level and be kept dry.

Hot forming, edge preparation, drilling, tapping and profile cutting are all routine operations. Thermal cutting leaves a hard, slightly decarburized edge on thicker plate, so the cut face is normally dressed or machined before welding.

Typical Applications

Boiler drums and shells operating with steam at roughly 300 - 350 degree C and pressures in the 9 - 12 MPa range.

High-pressure feedwater heaters and deaerator tanks, typically 250 - 300 degree C and 4 - 6 MPa.

Hydrotreating and hydrofining reactors with design conditions around 300 - 380 degree C and 4 - 8 MPa, together with the shells of shell-and-tube heat exchangers.

Regenerators and other vessels in catalytic cracking units handling mildly corrosive process media.

Storage tanks, gas holders, marine pressure vessels and general steam, air and oil pipelines.

Limits and Grade Selection Notes

A515 Gr 70 is a higher-temperature grade and is not intended for low-temperature impact service; where low-temperature toughness is required, an A516 plate with impact testing is the normal substitution. The grade is also not recommended for sour service, because a plain carbon-silicon steel has limited resistance to hydrogen-induced cracking in wet hydrogen sulfide environments and a HIC-tested grade is used instead. The nearest European parallel is the pressure vessel grade EN 10028-2 P265GH, but the chemistries and the test requirements differ, so the two should not be interchanged without a design review.

Frequently Asked Questions

Q: What is ASTM A515 Gr 70 used for?
It is used for boiler drums, shells and heads, high-pressure heaters, deaerator tanks, hot process vessels and storage tanks in power generation and petrochemical plants, where the service temperature is elevated but the design does not call for a low-alloy steel.

Q: Is A515 Gr 70 the same as A516 Gr 70?
They share the same minimum yield strength of 260 MPa and the same tensile range of 485 - 620 MPa, but they are different grades: A515 is a carbon-silicon plate for higher-temperature service, while A516 is a silicon-killed plate that can be ordered with low-temperature impact testing.

Q: What heat treatment is A515 Gr 70 supplied in?
Normalized is the usual condition for boiler and pressure vessel work; as-rolled, normalized and tempered, and quenched and tempered plate are also supplied when the order or the design code calls for them.

Q: Can A515 Gr 70 be used in sour service?
It is not recommended. A plain carbon-silicon steel has limited resistance to hydrogen-induced cracking in wet hydrogen sulfide environments, so a HIC-tested grade is used where sour service is specified.

Q: What thickness range is available?
Common supply covers 6 mm to 300 mm, in widths up to about 4050 mm and lengths up to 15000 mm, depending on the mill and the rolled stock.

Q: How is the plate certified?
Plates are supplied with a mill test certificate to EN 10204 3.1, and 3.2 certification or third-party inspection can be arranged when the project requires independent verification of the tests.