S355J2 and S355K2 are two sub-grades of the same EN 10025-2 structural steel family. They are produced from the same composition range, delivered with the same minimum yield strength of 355 MPa, and used for the same kinds of structure. The only real difference between them is a Charpy V-notch impact requirement: S355J2 must absorb at least 27 J at -20 °C, while S355K2 must absorb at least 40 J at the same temperature.
Same Standard, Same Base Grade
EN 10025-2 defines the base grade S355 together with the sub-grades JR, J0, J2 and K2, which differ only in impact testing. Every sub-grade keeps the S355 strength framework and the same chemistry limits; the letters and digits describe the impact test condition. J2 and K2 are the two lowest-temperature sub-grades of that standard, both tested at -20 °C, and they differ only in the minimum energy demanded from the test specimen.
Impact Test Requirements
| Sub-grade | Charpy test temperature | Minimum average energy, longitudinal | Typical delivery condition |
|---|---|---|---|
| S355JR | +20 °C | 27 J | as rolled |
| S355J0 | 0 °C | 27 J | as rolled or normalized rolled |
| S355J2 | -20 °C | 27 J | as rolled, normalized rolled or normalized |
| S355K2 | -20 °C | 40 J | normalized or normalized rolled |
K2 is therefore the tougher of the two low-temperature S355 grades. It is specified when the design code, the client specification or the fatigue and impact assessment calls for an energy absorption above the normal 27 J class, while the test temperature remains the same at -20 °C.
Chemical Composition of the J2 and K2 Qualities
Steel plate ordered as S355J2 or S355K2 is made to one and the same ladle analysis, and neither designation changes the composition limits. Phosphorus and sulphur are each capped at 0.025% for these two qualities, tighter than the 0.035% allowed for S355JR and S355J0, and nitrogen is limited to 0.012%. Silicon and copper are each held to 0.55% maximum. The tighter impurity control is what allows the plate to be impact tested at -20 °C, since phosphorus and sulphur are the elements that most damage toughness in the heat-affected zone of a weld.
Mechanical Properties by Thickness
| Nominal thickness (mm) | ReH min (MPa) | Rm (MPa) |
|---|---|---|
| ≤ 16 | 355 | 470-630 |
| > 16 - 40 | 345 | 470-630 |
| > 40 - 63 | 335 | 470-630 |
| > 63 - 80 | 325 | 470-630 |
| > 80 - 100 | 315 | 470-630 |
| > 100 - 150 | 295 | 450-600 |
| > 150 - 200 | 285 | 450-600 |
| > 200 - 250 | 275 | 450-600 |
| > 250 - 400 | 265 | 450-600 |
The table applies to both grades without distinction, which is the practical point of the comparison: the strength tables of S355J2 and S355K2 are identical over the whole thickness range. For plate thinner than 3 mm the tensile range is 510-680 MPa. Minimum elongation requirements also follow the base grade S355 and fall as thickness increases.
Delivery Condition and Availability
S355J2 is the more widely stocked grade and is available as rolled, controlled rolled, normalized rolled and normalized, in plate widths and lengths to suit most fabrication shops. S355K2 is more often ordered in the normalized or normalized rolled condition, because normalizing refines the grain structure and stabilises the higher energy absorption level in thick sections. Because availability is narrower for K2, project schedules should be planned around mill rolling programmes rather than on the assumption of ex-stock material. Both grades are stocked as cut-to-length plate and can be supplied with ultrasonic testing, edge preparation or shot blasting and priming when the purchase specification requires it.
Choosing Between S355J2 and S355K2
S355J2: the default choice for welded structural plate, building frames, bridge elements with normal impact demand, machine bases and general heavy fabrication.
S355K2: used for dynamically loaded and impact-exposed components such as crane and excavator parts, conveyor and crusher structures, cold-climate outdoor steelwork and offshore or marine structures.
Substitution rule: K2 may replace J2 where the specification allows a tougher grade, but J2 may not be used where K2 is written into the design or purchase specification, because the guaranteed energy absorption is lower.
Cost and lead time: J2 is normally cheaper and quicker to obtain; K2 carries a premium and a longer lead time that should be built into the order plan.
Frequently Asked Questions
Q: What is the difference between S355J2 and S355K2?
Only the Charpy impact requirement: 27 J minimum for S355J2 and 40 J minimum for S355K2, both tested at -20 °C on longitudinal specimens.
Q: Do S355J2 and S355K2 have the same chemical composition?
Yes. Both are produced to the same EN 10025-2 limits, with phosphorus and sulphur each capped at 0.025% and nitrogen at 0.012%.
Q: Do S355J2 and S355K2 have the same strength?
Yes. Minimum yield strength and tensile range tables are identical, starting at 355 MPa and 470-630 MPa for plate up to 16 mm.
Q: What does the K in S355K2 mean?
The letter identifies the higher energy class of impact test. K2 keeps the -20 °C test temperature of J2 but raises the minimum absorbed energy from 27 J to 40 J.
Q: Can S355J2 be used instead of S355K2?
Only if the engineering specification permits a lower guaranteed impact energy. Where K2 is specified, J2 does not comply.
Q: Which grade is suitable for low-temperature service?
Both are tested at -20 °C. For service below that temperature, a J2 or K2 plate with a normalized delivery condition, or an EN 10025-3 NL grade, should be considered.