What the Two Grades Have in Common
Q355NH and Q355GNH both belong to the Chinese weathering steel family defined in GB/T 4171, the standard for high atmospheric corrosion resistant structural steels. Both are low-alloy steels with a minimum yield strength of 355 MPa, both are supplied mainly as plate, and both are designed for structures that are left unpainted so that a dense, stable oxide layer forms and slows further corrosion.
Because the base strength class is identical, the two grades are often treated as one material at the design stage. That shortcut is only safe while the exposure conditions are ordinary. The moment the structure faces a more aggressive atmosphere, the difference in chemistry between NH and GNH becomes the deciding factor, and it is the corrosion allowance rather than the strength that governs the choice.
Chemical Composition: Where the Two Grades Separate
| Element, % | Q355NH | Q355GNH |
|---|---|---|
| Carbon, max | 0.16 | 0.12 |
| Silicon | max 0.50 | 0.20 to 0.75 |
| Manganese | 0.50 to 1.50 | max 1.00 |
| Phosphorus | max 0.030 | 0.07 to 0.15 |
| Sulphur, max | 0.030 | 0.020 |
| Copper | 0.25 to 0.55 | 0.25 to 0.55 |
| Chromium | 0.40 to 0.80 | 0.30 to 1.25 |
| Molybdenum, max | 0.30 | not listed for the grade |
| Titanium, max | 0.10 | not listed for the grade |
| Vanadium, max | 0.12 | not listed for the grade |
| Niobium, max | 0.06 | not listed for the grade |
The clearest separation is phosphorus. Q355NH keeps phosphorus at or below 0.030 percent, which suits welded construction because high phosphorus embrittles welds and the heat-affected zone. Q355GNH deliberately allows 0.07 to 0.15 percent phosphorus together with a wider chromium band, because phosphorus is one of the most effective elements for atmospheric corrosion resistance. The trade-off is weldability, which is why the GNH grade is normally reserved for bolted, riveted or lightly welded details and why its carbon and sulphur limits are held tighter than those of the NH grade.
Mechanical Properties Compared
| Property | Q355NH | Q355GNH |
|---|---|---|
| Minimum yield strength | 355 MPa | 355 MPa |
| Tensile strength | 516 to 670 MPa | 490 to 630 MPa |
| Minimum elongation | 26 percent | 26 percent |
| Carbon, max | 0.16 percent | 0.12 percent |
| Typical product form | Plate and strip for welded structures | Plate and strip for bolted or riveted structures |
Both grades sit in the same 355 MPa yield class and both are ductile enough for cold forming, so the strength table rarely decides the selection. Q355NH is the more weldable of the two because of its tightly capped phosphorus, while Q355GNH trades some weldability for a longer service life in aggressive atmospheres.
Why Q355GNH Resists Corrosion Better
Atmospheric corrosion resistance in weathering steel comes from a combination of alloying elements that promote a protective rust layer. Copper and chromium are the workhorses in both grades. Phosphorus is the differentiator: at the 0.07 to 0.15 percent level permitted in Q355GNH, it contributes strongly to the formation of a stable, low-porosity oxide film, which is why the GNH designation is described as high weathering steel. The wider chromium range of up to 1.25 percent adds further resistance in industrial and marine atmospheres.
The benefit appears only when the exposure permits wet and dry cycling and keeps the surface free of standing water, salt accumulation and abrasive wear. Structures that stay permanently wet, sit in chloride-rich spray zones, or are buried or immersed will not develop the protective layer, and in those conditions no weathering grade replaces a protective coating or a more highly alloyed material.
Applications and Grade Selection
Railway rolling stock, wagon bodies and hopper components that stay exposed and need low maintenance
Bridge girders, parapets and highway furniture where bare weathering steel is accepted by the design code
Transmission towers, poles and substation structures subject to weathering cycles
Shipping containers, port structures and cargo handling equipment
Offshore and onshore oil and gas equipment, including containers handling hydrogen sulphide bearing media where the design calls for a weathering grade
Industrial chimneys, silos, storage racks and general low-alloy structural steelwork
Selection rule of thumb: use Q355NH when the structure is welded and the atmosphere is moderate, and move to Q355GNH when the atmosphere is aggressive, when the design life is long, and when the connection method allows its higher phosphorus level. Where welding is unavoidable in a GNH design, the welding procedure has to be qualified for the grade rather than transferred from an NH procedure.
Frequently Asked Questions
Q: What is the main difference between Q355NH and Q355GNH?
Chemistry, and through it corrosion resistance. Q355GNH permits 0.07 to 0.15 percent phosphorus and a wider chromium range, which produces a more protective oxide layer, while Q355NH holds phosphorus at or below 0.030 percent for better weldability.
Q: Do the two grades have the same yield strength?
Yes. Both specify a minimum yield strength of 355 MPa, so strength is not the deciding factor. The tensile ranges quoted for the two grades differ, but both sit in the same high-strength low-alloy class.
Q: Can Q355GNH be welded?
It can be welded, but the elevated phosphorus content makes the weld and heat-affected zone more sensitive to cracking and embrittlement. Welding procedures and consumables have to be qualified for the grade, and bolted or riveted connections are usually preferred.
Q: Which grade should be used for a bridge?
It depends on the exposure and the connection design. Q355NH suits welded girder work in moderate atmospheres, while Q355GNH is chosen for aggressive environments and long design lives where the connection method tolerates its chemistry.
Q: Is Q355GNH more expensive?
Yes. The extra alloying and tighter control required to reach the high weathering performance make Q355GNH more costly per tonne than Q355NH, which is why it is specified only where the corrosion benefit is real.
Q: Does weathering steel ever need painting?
In clean, well-ventilated and freely draining exposures the surface is left bare. In chloride-rich, permanently damp, buried, immersed or heavily polluted conditions the protective layer will not form reliably, so a coating system or a different material is required.