ASTM A202 Grade A Cr-Mn-Si Alloy Steel Plate for Boilers and Pressure Vessels

Sep 18, 2025 Leave a message

Overview of ASTM A202 Grade A Cr-Mn-Si Steel Plate

ASTM A202 Grade A is a chromium-manganese-silicon (Cr-Mn-Si) alloy steel plate for welded boilers and other pressure vessels, covered by the specification ASTM A202/A202M. Grade A is the lower-strength grade of the specification: it has a controlled maximum carbon content of 0.17%, a minimum yield strength of 310 MPa and a specified tensile strength range of 515-655 MPa, equal to approximately 75-95 ksi.

The lower carbon level improves toughness and weldability compared with Grade B, which makes Grade A a common choice for welded shells, towers and heat exchange equipment where the design stress can be carried by a moderately strong plate and where fabrication quality is the dominant concern. Chromium and silicon provide elevated-temperature strength and resistance to oxidation, manganese contributes solid-solution strengthening, and the low carbon content keeps the heat-affected zone of welds ductile.

Chemical Composition of ASTM A202 Grade A

Element Limit, % (heat analysis)
Carbon (C), max 0.17
Silicon (Si) 0.54-0.90
Manganese (Mn) 0.97-1.52
Phosphorus (P), max 0.035
Sulfur (S), max 0.035

The specification applies the same silicon, manganese, phosphorus and sulfur limits to both grades; the essential difference between Grade A and Grade B is the carbon ceiling, 0.17% against 0.25%, together with the resulting strength levels. Product analysis tolerances apply when check analysis is requested, and the permitted residual element levels are stated in the specification for each element.

Mechanical Properties of ASTM A202 Grade A

Thickness, mm Yield strength, min, MPa Tensile strength, MPa Elongation, min, %
6-50 310 515-655 19
50-100 310 515-655 16

The tensile range of 515-655 MPa corresponds to 75-95 ksi. Minimum yield strength is 310 MPa throughout the tabulated thickness range, while the minimum elongation falls from 19% to 16% above 50 mm thickness. Impact testing is not mandatory under the base specification; Charpy V-notch testing at a purchaser-specified temperature is added as a supplementary requirement when the equipment is intended for low-temperature or otherwise critical duty.

Delivery Condition, Heat Treatment and Fabrication

AR - as-rolled supply, the standard delivery condition.

N - normalized, frequently specified for thick plate and for equipment where a uniform microstructure is required.

Q plus T - quenched and tempered, ordered when higher strength with adequate toughness is needed.

TMCP - thermo-mechanically controlled processing, used to improve toughness at a lower carbon equivalent.

Supplementary work - ultrasonic examination, Z-direction testing to Z15, Z25 or Z35, Charpy V-notch impact testing, third-party inspection, shot blasting and priming.

Grade A is readily formed, machined and welded. Flame cutting and cold forming are performed in the as-supplied condition, with stress relief after severe cold work. Welding uses low-hydrogen consumables matched to the plate strength; preheat is recommended above about 25 mm thickness and the interpass temperature is controlled to keep heat-affected zone hardness within code limits. Where post-weld heat treatment is specified, a typical cycle is 580-620 C for one hour per 25 mm of thickness, with the final cycle agreed between purchaser and manufacturer to suit the required strength and toughness.

Applications and Service Environments

Chemical reaction vessels, including ammonia synthesis towers and polymerisation reactors in fertiliser and chemical plants, where equipment such as a synthesis tower may operate at pressures around 30 MPa and temperatures around 450 C.

Petrochemical storage tanks, rectification towers and absorption towers in refining, including crude oil tanks and pressurised hydrotreating equipment.

Heat exchange equipment, such as shell-and-tube and plate heat exchangers, where shells and tube sheets must withstand repeated thermal cycling without weld cracking.

Metallurgical plant equipment, including blast furnace hot blast stove shells and autoclaves used in hydrometallurgical processing, where oxidation resistance and resistance to acid attack are important.

Service experience shows that Grade A performs well in the range from ambient temperature up to roughly 450 C, and it retains strength better than plain carbon pressure vessel steel of similar thickness because of its chromium and silicon content. It is not a cryogenic steel. Where service temperatures fall well below ambient, for example in liquefied natural gas storage at about -162 C, austenitic stainless steel or nickel-alloyed steels with verified low-temperature toughness are required, and impact-tested plate must be ordered with a test temperature appropriate to the design metal temperature.

Frequently Asked Questions

Q: What is ASTM A202 Grade A used for?
It is used for welded boilers, pressure vessels, storage tanks and heat exchangers, including chemical reaction vessels, refining towers and metallurgical plant equipment. Its low carbon content and good weldability suit fabricated equipment that operates at moderate to elevated temperature under internal pressure.

Q: How does Grade A differ from Grade B of the same specification?
Both grades are Cr-Mn-Si plates sharing the same silicon, manganese, phosphorus and sulfur limits. Grade A has a maximum carbon of 0.17%, a minimum yield strength of 310 MPa and a 515-655 MPa tensile range. Grade B allows up to 0.25% carbon with 325 MPa minimum yield and 587-760 MPa tensile strength.

Q: Can A202 Grade A be used at low temperature?
It is designed primarily for ambient to elevated-temperature pressure service, not for cryogenic duty. Applications such as liquefied natural gas storage at about -162 C require austenitic stainless steel or nickel-alloyed steel with verified low-temperature toughness, and any low-temperature use of Grade A must be supported by impact testing at the design metal temperature.

Q: What sizes are produced?
The specification tabulates properties for plate from 6 mm to 100 mm, and heavier plate can be supplied by agreement. Typical commercial widths range from 1500 mm to 4050 mm and lengths from 3000 mm to 15000 mm, allowing large shell plates to be cut with a minimum of welds.

Q: What delivery conditions and heat treatments are available?
As-rolled, normalized, quenched and tempered, and thermo-mechanically controlled processed plate can all be supplied. Normalizing is common for heavy plate or where a uniform structure is required, and stress relieving is applied after forming or welding when the design code demands it.

Q: Which designations are cited as equivalent to A202 Grade A?
Published cross-reference tables list designations such as E St E315, 18 MD 4.05, 16 Mo 6, 22.16.04 and 450M used in European national systems alongside this grade. Equivalence must be assessed against the applicable national standard, because composition ranges and test requirements differ between systems.