Overview of ASTM A202 Grade B Steel Plate
ASTM A202 Grade B is a chromium-manganese-silicon (Cr-Mn-Si) alloy steel plate covered by the standard specification ASTM A202/A202M for pressure vessel plates. The grade was developed for welded boilers and other pressure-bearing equipment, and it is normally selected where elevated-temperature strength, pressure containment and weldability must all be met in the same component. Grade B is the higher-strength grade of the specification: a high manganese level combined with chromium and silicon additions gives a minimum yield strength of 325 MPa and a tensile strength range of 587-760 MPa.
Because the plate is welded into shells, drums and heads, the specification limits phosphorus and sulfur to 0.035% maximum each so that the heat-affected zone remains sound after fabrication. Chromium raises elevated-temperature strength and oxidation resistance, manganese provides solid-solution strengthening together with useful hardenability, and silicon acts as a deoxidation element while improving resistance to scaling at temperature. The balanced analysis allows heavy sections to be formed, welded and stress relieved without an excessive loss of toughness.
Chemical Composition of ASTM A202 Grade B
| Element | Limit, % (heat analysis) |
|---|---|
| Carbon (C), max | 0.25 |
| Silicon (Si) | 0.54-0.90 |
| Manganese (Mn) | 0.97-1.52 |
| Phosphorus (P), max | 0.035 |
| Sulfur (S), max | 0.035 |
The values above are heat analysis limits taken from the material specification. When check analysis is requested by the purchaser, product analysis tolerances defined in ASTM A202/A202M apply, and the carbon, manganese and silicon results must still fall inside the permitted product ranges. Residual elements such as copper, nickel and chromium are kept low unless a specific analysis is agreed for a particular order.
Mechanical Properties of ASTM A202 Grade B
| Thickness, mm | Yield strength, min, MPa | Tensile strength, MPa | Elongation, min, % |
|---|---|---|---|
| 6-50 | 325 | 587-760 | 18 |
| 50-100 | 325 | 587-760 | 15 |
The tensile range of 587-760 MPa corresponds to approximately 85-110 ksi, which is the imperial basis from which the metric limits are derived. Minimum yield strength remains 325 MPa across the thickness range, while the minimum elongation requirement drops from 18% to 15% once the plate exceeds 50 mm, reflecting the lower through-thickness ductility of heavy sections.
Impact testing is not mandatory for the base specification. Charpy V-notch tests at a purchaser-specified temperature, together with a minimum absorbed energy requirement, are added as supplementary requirements when the equipment is intended for low-temperature service or for other critical duties. Tensile testing is performed on specimens taken in the direction of rolling, normally one test per heat treatment lot and thickness range.
Delivery Condition, Heat Treatment and Fabrication
AR - as-rolled supply, the default delivery condition.
N - normalized, common for thick plate or when a uniform ferrite-pearlite structure is required.
Q plus T - quenched and tempered when higher strength must be combined with toughness.
TMCP - thermo-mechanical control processing for improved toughness at a lower carbon equivalent.
Supplementary work - ultrasonic examination, Z-direction testing to Z15, Z25 or Z35, Charpy V-notch impact testing, third-party inspection, shot blasting and priming.
Fabrication follows normal practice for Cr-Mn-Si pressure vessel steel. Flame cutting, machining and cold forming are carried out in the as-supplied condition, and heavy cold forming is followed by stress relief. Welding uses low-hydrogen consumables matched to the plate strength; preheat is recommended for thickness above roughly 25 mm and the interpass temperature is controlled so that heat-affected zone hardness stays within the limits set by the design code. Where post-weld heat treatment is required, a typical cycle is 580-620 C for one hour per 25 mm of thickness, with the final cycle agreed between purchaser and manufacturer to suit the specified strength and toughness.
Applications and Service Environments
Boiler shells, drums, headers and steam piping in thermal power plants.
Pressure vessels and reactors in chemical and petrochemical plants.
Storage tanks, heat exchangers and separators in oil and gas projects.
Accumulators and other welded high-pressure process equipment.
The grade performs best in the range from ambient temperature up to about 450 C. In that window its chromium and silicon content provides useful resistance to oxidation and its strength retention is better than that of plain carbon pressure vessel steel of comparable thickness. For cryogenic duty or strongly hydrogen-charged service, grades with verified low-temperature toughness or additional qualification testing are normally selected instead.
Frequently Asked Questions
Q: What is the difference between ASTM A202 Grade A and Grade B?
Both grades are Cr-Mn-Si pressure vessel plates with the same silicon, manganese, phosphorus and sulfur limits. Grade A carries a maximum carbon of 0.17%, a minimum yield strength of 310 MPa and a tensile range of 515-655 MPa. Grade B permits up to 0.25% carbon and delivers 325 MPa minimum yield strength with 587-760 MPa tensile strength, so it is chosen for heavier or higher-pressure components.
Q: Is ASME SA202 Grade B the same material as ASTM A202 Grade B?
Yes. ASME SA202 Grade B is technically identical to ASTM A202 Grade B. The ASME designation applies when a vessel is designed and stamped to the ASME Boiler and Pressure Vessel Code, while the ASTM designation identifies the material specification itself. Chemical limits and mechanical properties are the same under both designations.
Q: What thickness can be supplied?
The specification tabulates property requirements over 6-100 mm. Heavier plate outside that range can be supplied by agreement, and commercial rolling programmes commonly cover 6-100 mm for boiler and pressure vessel work, with heavier sections produced for large drums and headers.
Q: Can the plate be supplied normalized or stress relieved?
Yes. As-rolled supply is standard, but the plate can be ordered normalized, stress relieved, or both. Above 50 mm thickness normalizing is frequent practice because it produces a more uniform microstructure and more consistent properties through the section.
Q: What inspection and testing is available?
Standard supply includes heat analysis plus tensile testing. Supplementary options include full-plate ultrasonic examination, Charpy V-notch impact testing, through-thickness Z-direction testing to Z15, Z25 or Z35, hardness surveys, dimensional checks and third-party inspection witnessed by the purchaser or its nominated agency.
Q: Which designations are commonly cited as equivalent to A202 Grade B?
Cross-reference tables for European national systems commonly list E St E315, 18 MD 4.05, 16 Mo 6, 22.16.04 and 450M alongside A202 Grade B. These designations are not interchangeable: composition ranges, impact requirements and delivery conditions differ, so equivalence must be assessed against the applicable national standard before any substitution is made.