P295GH and P355GH are normalized, non-alloy steel plates from the EN 10028-2 standard, primarily used for boilers, pressure vessels, and heat exchangers due to their excellent weldability and properties at elevated temperatures. The key difference lies in their strength: P295GH offers a minimum yield strength around 295 MPa (depending on thickness), while P355GH is stronger, typically featuring a minimum yield strength of 355 MPa (also varying with thickness), making it suitable for more demanding high-pressure applications.
Chemical Composition
P295GH Chemical Composition | |||||||
Grade | The Element Max (%) | ||||||
C | Si | Mn | P | S | Al(min) | N | |
P295GH | 0.08-0.20 | 0.40 | 0.80-1.50 | 0.025 | 0.015 | 0.020 | 0.012 |
Cr | Cu | Mo | Nb | Ni | Ti | V | |
0.30 | 0.30 | 0.08 | 0.020 | 0.30 | 0.03 | 0.02 | |
Carbon Equivalent: Ceq = 【C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15】%
P355GH Chemical Composition | |||||||
Grade | The Element Max (%) | ||||||
C | Si | Mn | P | S | Al(min) | N | |
P355GH | 0.10-0.22 | 0.60 | 1.10-1.70 | 0.025 | 0.015 | 0.020 | 0.012 |
Cr | Cu | Mo | Nb | Ni | Ti | V | |
0.30 | 0.30 | 0.08 | 0.040 | 0.30 | 0.03 | 0.02 | |
Mechanical Property
Grade |
| P295GH Mechanical Property | |||||
Thickness | Yield | Tensilmie | Elongation | Impact Energy(KV J) min | |||
P295GH | mm | Min Mpa | Mpa | Min % | -20° | 0° | +20° |
≤ 16 | 295 | 460-580 | 21 | 27 | 34 | 40 | |
16> to ≤40 | 290 | 460-580 | 21 | 27 | 34 | 40 | |
40> to ≤60 | 285 | 460-580 | 21 | 27 | 34 | 40 | |
60> to ≤100 | 260 | 460-580 | 21 | 27 | 34 | 40 | |
100> to ≤150 | 235 | 440-570 | 21 | 27 | 34 | 40 | |
150> to ≤250 | 220 | 430-570 | 21 | 27 | 34 | 40 | |
Grade |
| P355GH Mechanical Property | |||||
Thickness | Yield | Tensilmie | Elongation | Impact Energy(KV J) min | |||
P355GH | mm | Min Mpa | Mpa | Min % | -20° | 0° | +20° |
≤ 16 | 355 | 510-650 | 20 | 27 | 34 | 40 | |
16> to ≤40 | 345 | 510-650 | 20 | 27 | 34 | 40 | |
40> to ≤60 | 335 | 510-650 | 20 | 27 | 34 | 40 | |
60> to ≤100 | 315 | 490-630 | 20 | 27 | 34 | 40 | |
100> to ≤150 | 295 | 480-630 | 20 | 27 | 34 | 40 | |
150> to ≤250 | 280 | 470-630 | 20 | 27 | 34 | 40 | |
Minimum Yield Strength (MPa):
P295GH: 295 MPa (for thicknesses ≤ 16mm).
P355GH: 355 MPa (for thicknesses ≤ 16mm).
Tensile Strength (MPa):
P295GH: 460-580 MPa.
P355GH: 510-650 MPa (for thicknesses ≤ 60mm).
Applications: Both are used in boilers, pressure vessels, and heat exchangers, but P355GH's higher strength makes it more suitable for high-pressure/high-stress situations, often considered the more common choice.
Identification: The numbers "295" and "355" directly correspond to the minimum guaranteed yield strength in MPa for the base thickness.
Heat Treatment: P355GH often requires normalized heat treatment for its specified properties.
In essence, choose P355GH for higher strength and pressure resistance and P295GH for lower strength requirements, with P355GH generally being the stronger, more frequently used material in high-performance pressure equipment.