The EN 10025-6 Family and What the Letters Mean
EN 10025-6 covers flat products of high yield strength structural steels in the quenched and tempered condition. The designation combines four elements: S for structural steel, the number for the minimum yield strength in MPa, Q for the quenched and tempered delivery condition, and the toughness suffix, where Q is tested at -20 °C, QL at -40 °C and QL1 at -60 °C. S690Q and S890Q therefore differ only in strength level within the same specification framework, sharing the same delivery condition, the same mandatory impact testing regime and the same quench and temper production route.
Chemical Design
| Element, max % | C | Si | Mn | P | S | N | B | Cr | Mo | Ni | Cu | V | Nb | Ti | Zr |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| S890Q | 0.20 | 0.80 | 1.70 | 0.025 | 0.015 | 0.015 | 0.005 | 1.50 | 0.70 | 2.00 | 0.50 | 0.12 | 0.06 | 0.05 | 0.15 |
S890Q uses the same element set as S690Q but pushes the alloying towards the upper end of the permitted limits to develop the extra 200 MPa of yield strength. Nickel and chromium increase hardenability and toughness, molybdenum suppresses softening during tempering, boron improves response to quenching and titanium, niobium and vanadium control grain growth. Carbon remains capped, because raising carbon would harden the heat-affected zone during welding and reduce weldability faster than it raises strength. The carbon equivalent is defined in the standard and reported on the inspection certificate for every heat.
Mechanical Properties
| Grade | Thickness, mm | ReH min, MPa | Tensile, MPa | Elongation min, % | Charpy at -20 °C, min J |
|---|---|---|---|---|---|
| S690Q | 3-50 | 690 | 770-940 | 14 | 30 |
| S690Q | >50-100 | 650 | 760-930 | 14 | 30 |
| S690Q | >100-150 | 630 | 710-900 | 14 | 30 |
| S890Q | 3-50 | 890 | 940-1100 | 11 | 30 |
| S890Q | >50-100 | 830 | 880-1100 | 11 | 30 |
The step from S690Q to S890Q buys about 29% more yield strength, but elongation falls from 14% to 11% and the practical thickness ceiling drops from 150 mm to about 100 mm. Both grades require a minimum absorbed energy of 30 J at -20 °C, so toughness is not sacrificed in absolute terms, but the ductility margin available for cold forming and for accommodating fabrication tolerances is smaller in S890Q.
Choosing the Right Strength Level
S690Q is the standard solution for mobile crane booms, excavator arms, concrete pump booms, mining equipment, telescopic handlers, bridge strengthening works and heavy transport frames. It offers the best balance of strength, toughness, weldability and price in the quenched and tempered class, and it is produced in widths and lengths that suit large structural components.
S890Q is selected when the load is concentrated and the cross-section is squeezed by an external constraint: very long crane booms where tip deflection and transport weight are limiting, lift arms on large mining shovels, heavy vehicle chassis and suspension components, and specific retrofit applications where an existing envelope must be strengthened without changing geometry. The price premium and the tighter fabrication window mean it is normally specified only where the weight saving cannot be achieved another way.
Both grades are also available in QL and QL1 qualities for cold service, and both can be ordered with thickness-direction properties to EN 10164 in Z25 or Z35 classes for joints carrying through-thickness stress.
Fabrication, Welding and Quality Control
Thermal cutting of both grades produces a hardened edge on the cut face. Plasma, laser and waterjet cutting limit the affected layer; flame-cut edges on thick plate are ground back before welding or before the component enters fatigue service. Cold forming requires minimum bend radii that grow as the plate gets thicker and as the strength class rises, and hot forming above the tempering temperature is prohibited unless the component is re-quenched and tempered afterwards.
Welding a 690 MPa or 890 MPa quenched and tempered steel calls for a qualified procedure with a defined preheat, a maximum heat input, an interpass temperature ceiling and low-hydrogen consumables matched to the strength class. Undermatching consumables are often chosen deliberately, because a weld metal that is slightly softer than the parent metal reduces restraint cracking risk in thick joints; the design must then be checked for that lower weld strength. Heat-affected zone hardness limits are commonly verified by a hardness traverse on the procedure qualification test piece, and heat input is recorded by the welding machine during production.
Quality documentation covers heat analysis, product analysis, tensile testing, Charpy testing at the ordered temperature, hardness verification and dimensional inspection, issued as an inspection certificate to EN 10204. Ultrasonic examination to EN 10160 at an agreed class is standard practice for thick high-strength plate, since small internal discontinuities behave differently under high stress than in ordinary structural steel. Where the plate will be bent or welded in a critical joint, the delivered plate should be traced by heat number from the certificate to the finished component.
Frequently Asked Questions
Q: What is the difference between S690Q and S890Q?
A: The guaranteed minimum yield strength, 690 MPa against 890 MPa, together with a lower elongation requirement and a reduced thickness range for the stronger grade.
Q: Are both grades impact tested?
A: Yes. Both require a minimum Charpy V-notch absorbed energy of 30 J at -20 °C in the Q quality, with QL and QL1 qualities tested at -40 °C and -60 °C.
Q: How thick can S890Q be supplied?
A: The guaranteed properties are specified up to 100 mm, with the full 890 MPa yield in the 3-50 mm band.
Q: Is S890Q harder to weld than S690Q?
A: Yes. It needs tighter control of preheat, heat input and interpass temperature, and the heat-affected zone is more sensitive to softening and hardening.
Q: Why is the carbon content kept low in these grades?
A: Because carbon is the main driver of heat-affected zone hardness and cracking. Strength is obtained instead from alloying and the quench and temper treatment.
Q: Can S690Q be used instead of S890Q to save cost?
A: Often yes, if the design allows a slightly larger section or a reduced load. Where geometry is fixed and weight is critical, the higher grade is the practical solution.