S355J2 HSLA Sheet: Delivery States and Heat Treatment

Feb 28, 2024 Leave a message

S355J2-N-MTC-steel-plate.pdf

Grade Identity and Standard Basis

S355J2 is a weldable structural steel plate defined by EN 10025-2, the European standard for non alloy structural steels. The designation carries three pieces of information. The number 355 is the minimum yield strength in megapascals for the thinner portion of the thickness range. The J indicates a Charpy impact energy of 27 J and the figure 2 sets the test temperature at minus 20 degrees Celsius. Higher toughness variants in the same strength class, such as K2 at minus 20 degrees Celsius with 40 J, are also available where a project demands a greater energy absorption level.

In Chinese practice the closest equivalent is the Q355 grade family of GB/T 1591-2018, and projects that mix European and Chinese specifications must compare both the strength requirement and the impact requirement, not only the yield strength, since the energy level and the test temperature are what distinguish otherwise similar grades.

Delivery States and What They Mean

The same S355J2 grade can be supplied in several delivery states, and the state determines the microstructure that the fabricator receives. The mechanical property requirements of the standard must be met in each case, but the way those properties behave during fabrication differs.

Delivery state Production route Practical consequence
Hot rolled Rolled above the recrystallisation temperature without further treatment Standard structural supply, suitable for general fabrication
Normalised Heated to the normalising temperature and air cooled Uniform, fine grained structure with stable toughness
Normalised rolled Final deformation controlled within a defined temperature range Properties equivalent to normalising without an extra reheat
Thermomechanically rolled Controlled rolling with accelerated cooling Fine grained, high toughness, but sensitive to hot work

Hot rolling refines nothing beyond the effect of deformation and cooling: the ingot or billet is reheated and rolled, then cut to size and levelled. Controlled rolling adjusts the heating temperature, the rolling temperature and the deformation schedule to control the way austenite transforms, which refines the structure and improves the balance of strength and toughness. Normalising rolling produces a condition equivalent to normalising by controlling the finishing pass, so the plate achieves the same specified mechanical values as a normalised plate without a separate heat treatment cycle.

Heat Treatment Practice

Normalising heats the plate to a temperature above the transformation range and then allows it to cool in air, which produces a finer, more homogeneous structure than the as rolled condition and gives a consistent result through the thickness. The structure that results is tougher and more uniform, which suits components that must combine strength with impact resistance.

Normalising temperature: typically in the range of 880 to 920 degrees Celsius, followed by air cooling.

Stress relief: applied after welding or heavy machining, generally around 550 to 600 degrees Celsius, with the soak temperature kept below the point at which the properties of the plate begin to deteriorate.

Quenching and tempering: not part of the S355J2 specification for structural plate and not used to make the grade.

Thermomechanically rolled plate: should not be normalised, because the reheat removes the fine grained structure produced by the rolling schedule.

During stress relief the soak temperature and the cooling rate after the treatment both matter. A temperature that is too high softens the plate and reduces the impact energy, while an uncontrolled cooling rate in a heavy fabrication can reintroduce residual stress. The treatment cycle is therefore recorded and applied to the whole fabrication in a controlled furnace whenever a project specifies it.

Mechanical Properties and Application Range

S355J2 is specified with a minimum yield strength of 355 MPa for thickness up to 16 mm, reducing with thickness, a tensile strength of 470 to 630 MPa, and a minimum elongation of 22 percent. The J2 designation guarantees a minimum Charpy absorbed energy of 27 J at minus 20 degrees Celsius.

The grade is used for welded structures in general engineering, for bridges and crane structures in temperate and cold conditions, for storage tanks, for industrial buildings, for transport equipment and for machinery frames. It is a first choice for projects that need a normalised or normalised rolled material with a defined low temperature toughness rather than a plain as rolled plate.

Common Misconceptions and Quality Control

A persistent misconception is that any S355 plate can be normalised after rolling to improve it. That holds for hot rolled plate, but thermomechanically rolled plate loses its properties in the process. A second misconception is that the J2 suffix only indicates strength: the suffix is a toughness designation, and a design that requires 27 J at minus 20 degrees Celsius cannot be satisfied by a plate specified without the toughness classification.

Quality control covers chemical analysis per heat, tensile testing per test unit, impact testing at the specified temperature and dimensional inspection of thickness, width, length and flatness. Where a project requires verification of the delivery state, the certificate records the treatment route, and additional ultrasonic examination or through thickness testing can be ordered for restrained welded connections.

Frequently Asked Questions

Q: What does J2 mean in S355J2?

A: The J denotes a minimum Charpy impact energy of 27 J and the 2 sets the test temperature at minus 20 degrees Celsius.

Q: What is the minimum yield strength?

A: 355 MPa for thickness up to 16 mm, with the required value decreasing as plate thickness increases.

Q: Can thermomechanically rolled plate be normalised?

A: No. Normalising a thermomechanically rolled plate destroys the fine grained structure responsible for its properties.

Q: What stress relief temperature is used after welding?

A: Typically around 550 to 600 degrees Celsius, with the soak time and cooling rate controlled so that impact properties are not reduced.

Q: Is S355J2 the same as Q355?

A: The two are similar strength classes in different standards, but the impact requirement and test temperature must be compared before the materials are treated as equivalent.

Q: Which delivery state should be ordered?

A: Choose according to the fabrication route and the design requirement: hot rolled for general work, normalised or normalised rolled where consistent toughness through the thickness is needed.