P295GH steel plate is a low alloy steel plate for high temperature pressure vessels. P295GH steel plate has good heat resistance and pressure resistance and is often used to manufacture containers and boiler equipment under high temperature and high pressure. Comply with the requirements of European standard EN10028 and German standard DIN17155. P295GH steel plates are usually hot rolled and are available in different thicknesses and sizes. When using P295GH steel plate, you need to pay attention to its applicable working temperature and pressure range to ensure safe and reliable use.
Chemical Composition of EN 10028 – P295GH:
| C | 0.08 to 0.20 | Cr | ≤0.30 |
| Si | ≤0.40 | Cu | ≤0.30 |
| Mn | 0.90 to 1.50 | Mo | ≤0.08 |
| P | 0.025 | Nb | ≤0.020 |
| S | 0.015 | Ni | ≤0.30 |
| Al | ≤0.020 | Ti | 0.03 |
| N | ≤0.012 | Vi | ≤0.02 |
Mechanical Properties of EN 10028 – P295GH:
| Type | Thickness (mm) | Yield Strength MPa (min) |
Tensile Strength MPa |
Elongation % (min) |
Impact Energy (KV J) (min) |
|||
| -20° | 0° | +20° | ||||||
| Normalized | ≤ 16 | 295 | 460 - 580 | 21 | 27 | 34 | 40 | |
| 16> to ≤40 | 290 | 460 - 580 | 21 | 27 | 34 | 40 | ||
| 40> to ≤60 | 285 | 460 - 580 | 21 | 27 | 34 | 40 | ||
| 60> to ≤100 | 260 | 460 - 580 | 21 | 27 | 34 | 40 | ||
| 100> to ≤150 | 235 | 440 - 570 | 21 | 27 | 34 | 40 | ||
| 150> to ≤250 | 220 | 430 - 570 | 21 | 27 | 34 | 40 | ||