What 15CrMo Plate Is
15CrMo is a low alloy chromium molybdenum steel defined by GB/T 3077-2015, the Chinese standard for alloy structural steels. The designation reports the nominal carbon content, 0.15 percent, and the main alloying additions, chromium and molybdenum. In plate form the grade is used for components that operate at elevated temperature and under pressure, which is why it also appears in the pressure vessel family as 15CrMoR under GB/T 713-2014 with a slightly modified analysis and a guaranteed minimum elevated temperature yield strength.
The value of chromium and molybdenum in a steel of this type lies in what they do at temperature rather than at room temperature. Chromium raises resistance to oxidation and to certain corrosive media, while molybdenum strongly increases the resistance of the steel to softening and creep at high temperature. Together they also improve resistance to hydrogen attack, which is the internal decarburisation and fissuring that occurs when steel is exposed to hydrogen at elevated temperature and pressure.
Chemical Composition and Heat Treatment
The composition of 15CrMo is tightly banded because the grade is heat treated after forming and the analysis determines how the section responds to that treatment.
| Element | Content (percent) | Role |
|---|---|---|
| Carbon | 0.12 to 0.18 | Strength and hardenability |
| Silicon | 0.17 to 0.37 | Deoxidation, solid solution strengthening |
| Manganese | 0.40 to 0.70 | Strength and toughness |
| Chromium | 0.80 to 1.10 | Oxidation and corrosion resistance, elevated temperature strength |
| Molybdenum | 0.40 to 0.55 | Creep strength, resistance to hydrogen attack |
| Phosphorus and sulphur | restricted residuals | Cleanliness and toughness control |
Plate is normally supplied in the normalised and tempered condition. Annealing is also offered when heavy machining is required before final heat treatment, and an annealed plate has a maximum Brinell hardness that keeps it machinable with conventional tooling. Because molybdenum raises hardenability, cooling rate control during normalising is important in heavy plate, and the mill records the treatment cycle with the plate identification.
Mechanical Properties
Room temperature requirements for 15CrMo are a tensile strength of 440 to 640 MPa, a minimum yield strength of 295 MPa and a minimum elongation of 22 percent. The annealed condition carries a hardness ceiling that keeps the plate machinable, while the normalised and tempered condition delivers the strength and toughness combination used in service. Where the pressure vessel grade 15CrMoR is ordered, the certificate additionally reports elevated temperature yield strength values, which are the values used by the designer at the working temperature of the vessel.
For high temperature design the engineer works from the creep and stress rupture data for the grade rather than from room temperature tensile values, because at the upper end of its service range the allowable stress is governed by time dependent behaviour. This is why the plate is ordered against a standard that includes elevated temperature property requirements rather than a general structural specification.
Service Applications
15CrMo plate is used in the petroleum, chemical, power generation and nuclear sectors, primarily for pressure retaining components and for parts that combine mechanical load with elevated temperature. Typical items include steam drums and headers, superheater supports, reactor and heat exchanger shells, hydrocracker and hydrotreater components, high pressure steam piping attachments, and forged or rolled rings for turbine and valve bodies.
Outside the pressure vessel field the grade is also used for mechanical parts that need strength, hardness and wear resistance with some elevated temperature capability, such as high strength bolts, shafts, gears and heavy duty tooling. In those duties the plate is usually purchased for machining and then heat treated to the final property level by the component manufacturer, so the delivered plate is supplied in a machinable condition with a controlled analysis.
Fabrication Notes and Misconceptions
Fabrication of 15CrMo follows the practice used for alloy pressure vessel steels. Cutting is done by flame, plasma or waterjet, with preheat applied above roughly 20 to 25 mm thickness. Cold forming is preferred over hot forming, and any hot forming operation must be followed by a full normalising and tempering treatment because the elevated temperature work destroys the refined structure. Welding uses matching chromium molybdenum consumables, low hydrogen practice and preheat in the range of 150 to 200 degrees Celsius, with post weld heat treatment applied where the procedure requires it.
A common misunderstanding is that a chromium molybdenum plate is inherently corrosion resistant in the same way as a stainless steel. It is not. Chromium at around 1 percent improves oxidation resistance and hydrogen resistance, but the grade still requires protection in aggressive aqueous environments. Another frequent error is to treat 15CrMo and 15CrMoR as fully interchangeable: the two are related but the pressure vessel version carries additional elevated temperature and impact requirements, and the purchase order should state which specification applies.
Frequently Asked Questions
Q: What is the difference between 15CrMo and 15CrMoR?
A: 15CrMo follows the alloy structural steel standard GB/T 3077-2015, while 15CrMoR is the pressure vessel plate grade under GB/T 713-2014 with additional elevated temperature and toughness requirements.
Q: What is the maximum service temperature?
A: The grade is used in high temperature service up to around 550 degrees Celsius, with allowable stresses taken from the elevated temperature data in the applicable standard.
Q: In what condition is the plate delivered?
A: Normalised and tempered is the standard supply condition, and an annealed condition is available when the plate must be machined before final heat treatment.
Q: What preheat is used for welding?
A: Preheat in the range of 150 to 200 degrees Celsius with matching chromium molybdenum low hydrogen consumables is normal for this steel.
Q: Can 15CrMo plate be hot formed?
A: Hot forming is possible but must be followed by normalising and tempering, since the working temperature removes the benefit of the original heat treatment.
Q: Is 15CrMo a stainless steel?
A: No. Its chromium content is far below the stainless threshold, so it resists oxidation and hydrogen attack at temperature but is not corrosion resistant in aggressive aqueous media.