S500Q and S550Q: Two Strength Levels of Q&T Plate
S500Q and S550Q are high strength structural steel plates supplied in the quenched and tempered condition under EN 10025-6. They are used for welded and bolted structures that must carry heavy loads with a low self weight, and both grades combine a high yield point with enough toughness to resist brittle fracture in service.
The designation is systematic. S indicates structural steel, 500 and 550 are the minimum yield strengths in MPa, and Q marks the quenched and tempered delivery condition, which implies a low temperature impact requirement as part of the grade definition. S550Q is the stronger of the two, while S500Q offers slightly better ductility and a somewhat wider choice of thickness ranges.
Quenching from the austenitizing temperature followed by tempering develops a fine tempered martensitic or bainitic structure. The alloy design stays lean: carbon is limited to 0.20 percent, and strength is obtained through manganese, chromium, molybdenum, nickel and microalloying rather than through carbon content, which keeps weldability manageable.
Chemical Composition of Both Grades
EN 10025-6 applies one set of maximum values to S500Q and S550Q, so the two grades are not distinguished by chemistry. The limits are shown below.
| Element | Max, % | Purpose |
|---|---|---|
| Carbon (C) | 0.20 | Strength; restricted for welding |
| Silicon (Si) | 0.80 | Deoxidation |
| Manganese (Mn) | 1.70 | Hardenability and toughness |
| Phosphorus (P) | 0.025 | Impurity control for toughness |
| Sulfur (S) | 0.015 | Impurity control for cleanliness |
| Nitrogen (N) | 0.015 | Controlled with aluminium and titanium |
| Boron (B) | 0.005 | Hardenability |
| Chromium (Cr) | 1.50 | Hardenability and tempering resistance |
| Copper (Cu) | 0.50 | Residual control |
| Molybdenum (Mo) | 0.70 | Tempering resistance |
| Niobium (Nb) | 0.06 | Grain refinement |
| Nickel (Ni) | 2.0 | Low temperature toughness |
| Titanium (Ti) | 0.05 | Nitrogen fixation |
| Vanadium (V) | 0.12 | Precipitation strengthening |
| Zirconium (Zr) | 0.15 | Inclusion control |
Mechanical Properties Compared by Thickness
Strength falls as plate thickness increases, because the cooling rate at the core during quenching is slower. The guaranteed values below are the ones that must be met at each thickness range.
| Grade and thickness, mm | Min yield, MPa | Tensile, MPa | Min elongation, % |
|---|---|---|---|
| S500Q, 3 < t <= 50 | 500 | 590-770 | 17 |
| S500Q, 50 < t <= 100 | 480 | 590-770 | 17 |
| S500Q, 100 < t <= 150 | 440 | 540-720 | 17 |
| S550Q, 3 < t <= 50 | 550 | 640-820 | 16 |
| S550Q, 50 < t <= 100 | 530 | 640-820 | 16 |
| S550Q, 100 < t <= 150 | 490 | 590-770 | 16 |
Impact testing is carried out at -20 °C with a minimum absorbed energy of 30 J for both grades. The elongation requirement is 17 percent for S500Q and 16 percent for S550Q, a small but predictable consequence of the higher strength level of the 550 grade.
Strength, Ductility and Design Consequences
The step from 500 MPa to 550 MPa minimum yield strength is a ten percent gain in design resistance, and it is usually taken either as a weight saving or as additional load capacity. In practice a designer can keep the same section and increase the allowable load, or reduce the section and keep the load, which lowers steel consumption, transportation cost and foundation loads.
The trade off appears in ductility and toughness margins. S550Q has a lower minimum elongation, a narrower tensile range and a higher strength to toughness ratio, so it is chosen where stress levels are genuinely high and where welding procedures are well controlled. For structures dominated by stiffness rather than stress, the 500 grade gives the same deflection behaviour at lower cost and with more fabrication tolerance.
Both grades are covered by EN 10025-6, and comparable grades appear in ISO 630-4 for quenched and tempered structural steels, which helps when projects need cross standard documentation.
Fabrication and Welding Notes
Preheat at 100-150 °C for thicknesses above 20 mm, and keep the interpass temperature below about 250 °C.
Use low hydrogen consumables of matched strength; for the 550 grade a slightly undermatching filler is often accepted to improve toughness.
Limit heat input and avoid high deposition rates that produce a soft heat affected zone in quenched and tempered plate.
Post weld heat treatment is generally not required; if specified, hold below the mill tempering temperature to avoid loss of strength.
Thermal cutting edges should be cleaned of dross and lightly ground before welding, especially on thick sections.
Applications
S500Q: bridges, building frames, crane structures, heavy transport equipment and general high strength welded fabrication.
S550Q: heavy duty lifting equipment, mining and port machinery, long span girders, and pressure bearing support structures where stress levels are high.
Both grades: plant construction and industrial structures that combine high strength to weight ratio with reliable toughness.
Frequently Asked Questions
Q: What is the main difference between S500Q and S550Q?
The minimum yield strength: 500 MPa for S500Q and 550 MPa for S550Q. The tensile range and elongation requirement also rise and fall accordingly.
Q: Do the two grades have different chemical compositions?
No. Both are subject to the same EN 10025-6 maximum limits; the property difference comes from composition balance within those limits and from heat treatment.
Q: At what temperature is impact testing performed?
Both grades are tested at -20 °C with a minimum absorbed Charpy energy of 30 J, which covers most outdoor structural service.
Q: Can S550Q replace S500Q to save weight?
Often yes, provided fatigue, buckling, weldability and stiffness checks are repeated, because a thinner section may govern deflection rather than stress.
Q: Why is the elongation lower for S550Q?
Higher strength usually costs some ductility, so EN 10025-6 requires 16 percent minimum elongation for the 550 grade against 17 percent for the 500 grade.
Q: Is heat treatment after welding allowed?
It is allowed only when a project requires it, and the holding temperature must stay below the tempering temperature used in production to prevent a drop in strength.