P690Q vs P690QH: Quenched and Tempered Pressure Steel Plate Differences

Nov 27, 2025 Leave a message

P690Q and P690QH: High Strength Pressure Plate Grades

P690Q and P690QH are quenched and tempered steel plate grades for pressure purposes with a nominal minimum yield strength of 690 MPa. Both belong to the same strength class of the European pressure steel system, which means they are delivered in the quenched and tempered condition and are used where a combination of very high strength, moderate weight and reliable toughness is needed, such as heavy walled vessels, penstocks, hydropower components, large container structures and high pressure gas storage.

The designation follows the same logic as the normalized pressure grades. The letter P marks pressure purposes, 690 is the minimum yield strength in MPa, and Q indicates that the plate is quenched and tempered rather than normalized. The additional letter H identifies the variant that carries mandatory impact testing together with tighter impurity control and the supplementary quality requirements applied to plates used in demanding container and heavy fabrication work.

The Main Difference Between P690Q and P690QH

P690Q is the base quenched and tempered grade of the 690 MPa strength class. P690QH is the enhanced variant of the same strength class: it adds a specified Charpy impact test requirement, applies stricter limits to phosphorus and sulphur, and is the grade normally ordered when the plate must also satisfy container plate requirements such as ultrasonic flaw detection and through thickness performance.

Item P690Q P690QH
Strength class 690 MPa minimum yield 690 MPa minimum yield
Delivery condition Quenched and tempered Quenched and tempered
Charpy impact testing As specified for the grade Mandatory, at the grade test temperature
Maximum phosphorus 0.025 % 0.025 %
Maximum sulphur 0.015 % 0.015 %
Typical extra requirements Standard ultrasonic testing on request Flaw detection and thickness direction performance for containers
Zirconium treated option Not listed Zirconium up to 0.15 % listed

In practice the choice is driven by the inspection and toughness regime of the project rather than by strength, because the guaranteed yield and tensile values of the two variants are the same across the thickness range.

Chemical Composition

Both grades are low carbon, micro-alloyed quenched and tempered steels. The table below gives the maximum element contents applied to the heat analysis.

Element P690Q P690QH
Carbon, C 0.20 % max 0.20 % max
Silicon, Si 0.80 % max 0.80 % max
Manganese, Mn 1.70 % max 1.70 % max
Phosphorus, P 0.025 % max 0.025 % max
Sulphur, S 0.015 % max 0.015 % max
Nitrogen, N 0.015 % max 0.015 % max
Boron, B 0.005 % max 0.005 % max
Chromium, Cr 1.50 % max 1.50 % max
Copper, Cu 0.30 % max 0.30 % max
Molybdenum, Mo 0.70 % max 0.70 % max
Niobium, Nb 0.06 % max 0.06 % max
Nickel, Ni 2.50 % max 2.50 % max
Titanium, Ti 0.05 % max 0.05 % max
Vanadium, V 0.12 % max 0.12 % max
Zirconium, Zr Not specified 0.15 % max

Boron is restricted to 0.005 % maximum because even small boron additions strongly influence hardenability and weldability. Carbon equivalent is controlled by the familiar relationship Ceq = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15, expressed in percent, and a low value is essential for crack free welding of thick sections.

Mechanical Properties by Thickness

Strength decreases as thickness grows because the quenching rate at the core of a heavy plate is slower. Both variants share the following values.

Nominal thickness Minimum yield strength Tensile strength Minimum elongation
6 - 50 mm 690 MPa 770 - 940 MPa 14 %
Over 50 - 100 mm 670 MPa 770 - 940 MPa 14 %
Over 100 - 150 mm 630 MPa 720 - 900 MPa 14 %

For P690QH the yield strength steps are 690 MPa up to 50 mm, 670 MPa above 50 mm up to 100 mm and 630 MPa above 100 mm, with the tensile band shifting from 770 to 940 MPa for plate up to 100 mm to 720 to 900 MPa for heavier plate. The higher strength compared with P460 grades allows a designer to reduce wall thickness substantially, which lowers fabrication weight and cost but demands more attention to stress concentration, fatigue detail and welding procedure qualification.

Welding, Forming and Inspection

Quenched and tempered 690 MPa plate is welded with matching strength consumables and a controlled heat input. The heat affected zone softens if the heat input is too high, and hardens if it is too low with insufficient preheat, so the qualified procedure normally fixes a band of heat input, a minimum preheat and a maximum interpass temperature.

Preheat is generally required for thick sections and low ambient shop temperature.

Heat input is limited to protect the tempered microstructure of the base metal and the heat affected zone.

Post weld heat treatment, where applied, is carried out below the original tempering temperature.

Ultrasonic testing to detect internal discontinuities is standard for pressure and container applications.

Through thickness tensile testing is used to confirm resistance to lamellar tearing in restrained joints.

Cold forming is possible within generous radii, and hot forming requires re-quenching and tempering afterwards to restore the guaranteed properties. Because the strength class is high, edges should be machined or ground smooth before service to avoid notch effects.

Selecting Between P690Q and P690QH

Choose P690Q when the design demands 690 MPa yield strength with standard delivery testing and normal ultrasonic examination. Choose P690QH when the application is a container, a heavily restrained fabrication or a pressure component for which flaw detection and thickness direction ductility are mandatory, since the H variant is the grade intended to satisfy those supplementary requirements. In both cases the ordering enquiry should state the thickness, the impact test temperature, the ultrasonic testing class and the required through thickness properties, because these variables, not the base chemistry, determine the delivered plate.

Frequently Asked Questions

Q: Is P690QH stronger than P690Q?
No. Both belong to the same 690 MPa strength class and have identical minimum yield strength and tensile strength values for the same thickness.

Q: What does the H mean in P690QH?
It identifies the enhanced variant of the quenched and tempered grade, supplied with specified impact testing and the supplementary inspection and through thickness quality requirements used for container plate.

Q: Why is boron limited to 0.005 %?
Boron raises hardenability sharply even in very small amounts, which would harm weldability and toughness in thick quenched and tempered plate.

Q: How is carbon equivalent calculated for these grades?
By the expression Ceq = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15, with all element contents taken from the heat analysis.

Q: Can the yield strength be maintained in heavy plate?
Yes, but it steps down with thickness, from 690 MPa up to 50 mm to 670 MPa up to 100 mm and 630 MPa above 100 mm.

Q: Are these plates easy to weld?
They weld reliably with a qualified procedure that controls preheat, heat input and interpass temperature; uncontrolled heat input degrades the tempered structure.