ASTM A203 Grade A and Grade B are nickel-alloy steel plates for welded pressure vessels, differing mainly in their nickel content and mechanical properties, with Grade B offering higher minimum yield strength (around 275 MPa) compared to Grade A (around 255 MPa), making Grade B suitable for more demanding applications, both generally featuring about 2% nickel for low-temperature service, though specific chemistries and heat treatments vary slightly by manufacturer.
Mechnical property for A203 Grade B steel plate
|
Mechanical Property of A203 Grade A steel plate |
A203 Grade A |
|
Tensile strength, kis [MPa] |
65-85 [450-585] |
|
Yield strength, min, kis [MPa] |
37 [255] |
|
Elongation in 8 in. [200 mm], min, % |
15 |
|
Elongation in 2 in. [50 mm], min, % |
19 |
Mechnical property for A203 Grade B steel plate
|
Mechanical Property of A203 Grade B steel plate |
A203 Grade B |
|
Tensile strength, kis [MPa] |
70-90[485-620] |
|
Yield strength, min, kis [MPa] |
40 [275] |
|
Elongation in 8 in. [200 mm], min, % |
17 |
|
Elongation in 2 in. [50 mm], min, % |
21 |
Chemical composition for A203 Grade A steel plate
|
Grade |
The Element Max (%) |
||||
|
C |
Si |
Mn |
P |
S |
|
|
A203 Grade A |
0.17 |
0.13-0.45 |
0.78-0.88 |
0.035 |
0.035 |
Chemical composition for A203 Grade B steel plate
|
Grade |
The Element Max (%) |
||||
|
C |
Si |
Mn |
P |
S |
|
|
A203 Grade B |
0.17 |
0.13-0.45 |
0.78-0.88 |
0.035 |
0.035 |
Key Differences & Similarities
Material Type: Both are nickel-alloy steels (2% nickel steels) specified by ASTM for pressure vessels.
Application: Used in oil, gas, chemical, and power industries for reactors, heat exchangers, and storage tanks.
Strength: Grade B has slightly higher minimum yield strength and tensile strength than Grade A.
Nickel Content: Typically around 2.0% to 3.0% nickel, tailored for low-temperature toughness.
Heat Treatment: Often requires normalization to meet mechanical properties.
ASTM A203 Grade A: Lower strength, acceptable for less demanding pressure vessel parts.
ASTM A203 Grade B: Higher strength (min yield ~275 MPa), making it more common for higher pressure/temperature vessels.