ABS FH36 marine steel plates that are widely used in the construction of ships and other marine structures. The grade is specified by the American Bureau of Shipping (ABS) and are renowned for their excellent strength, toughness, and weldability.
|
ABS FH36 high Strength Chemical Composition |
|||||||
|
Grade |
The Element Max (%) |
||||||
|
C |
Si |
Mn |
P |
S |
Al |
N |
|
|
ABS FH36 |
0.16 |
0.1-0.50 |
0.90-1.6 |
0.025 |
0.025 |
0.015 |
0.009 |
|
Nb |
V |
Ti |
Cu |
Cr |
Ni |
Mo |
|
|
0.02-0.05 |
0.05-0.10 |
0.02 |
0.35 |
0.2 |
0.8 |
0.08 |
|
Crack Sensitivity: Pcm = (C+Si/30+Mn/20+Cu/20+Ni/60+Cr/20+Mo/15+V/10+5B)%
Carbon Equivalent: Ceq = 【C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15】%
|
ABS FH36 high strength property |
|||||||
|
Grade |
|
Mechanical Property |
Charpy V Impact Test |
||||
|
Thickness |
Yield |
Tensile |
Elongation |
Degree |
Energy 1 |
Energy 2 |
|
|
ABS FH36 |
mm |
Min Mpa |
Mpa |
Min % |
-60 |
J |
J |
|
t≤50 |
355 |
490-620 |
21% |
24 |
34 |
||
|
50<t≤70 |
355 |
490-620 |
21% |
27 |
41 |
||
|
70<t≤100 |
355 |
490-620 |
21% |
34 |
50 |
||
|
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
|||||||
ABS FH36 steel plates are typically supplied in a normalized or quenched and tempered condition. Normalized heat treatment involves heating the steel to a specific temperature and then allowing it to cool slowly, which improves its internal structure and mechanical properties. Quenched and tempered steel, on the other hand, undergoes a more rigorous heat treatment process that involves rapid cooling (quenching) followed by tempering to achieve desired strength and toughness levels.
Impact testing is an essential part of the quality control process for ABS FH36 steel plates. This testing involves subjecting the steel to low-temperature impact forces to assess its toughness and ability to withstand sudden loads. The results of these tests ensure that the steel plates meet the strict standards set by the ABS for use in marine applications.