A517GrQ is a high-strength quenched and tempered steel plate, a type of killed steel, with ultra-high strength, uniform and good low-temperature toughness and low crack sensitivity requirements.
A517GrQ steel plate grade indication:
"A": indicates American standard alloy steel;
"517": indicates that the yield strength of the steel plate is 517Mpa.
"Gr": Abbreviation for Grade.

A517GrQ High Strength Plate Chemical Composition:
Standards | C | Mn | P | S | Si | Ni | Cr | Mo | V |
| A517GrQ | 0.12-0.23 | 0.95-1.30 | 0.025 | 0.025 | 0.15-0.35 | 1.20-1.50 | 1.0-1.5 | 0.4-0.6 | 0.03-0.08 |
A517GrQ Steel Plate Mechanical Properties:
Standards | Tensile strength, Mpa | Yield strength, Mpa | Elongation in 2mm |
| A517GrQ | 725-930 | 620 | 14 |
A517GrQ Steel Plate Production and Cutting Process Flow
Production Context:
With the development of offshore oil and gas exploration and extraction into deeper waters, self-elevating marine platforms impose increasingly high demands on the strength, plasticity, toughness, and thickness of rack steel plates. For example, a 350-foot self-elevating marine platform typically requires rack steel plates with a thickness of 152.4 mm, a yield strength of 690 MPa, a tensile strength in the range of 790–930 MPa, an elongation of 14%, and a Charpy impact energy of 69 J at low temperatures (typically at -40°C at 1/4 thickness of the plate and -27°C at the core, i.e., 1/2 thickness of the plate). To meet these requirements, the industry has been committed to developing heavy-thickness rack steel plates. For instance, the invention patent with publication number CN102345045A discloses a marine platform rack steel plate A514GrQ and its manufacturing method.
A method for directly producing heavy-thickness rack steel plates using continuous casting slabs. Furthermore, the rack steel plate has a thickness of 114–152.4 mm and is directly manufactured using continuous casting slabs. The resulting yield strength is 690 MPa, tensile strength is 790–930 MPa, elongation is 19%, Z-direction performance (reduction of area) is 35%, Charpy impact energy at 1/4 thickness of the plate at -40°C is >100 J, and Charpy impact energy at 1/2 thickness of the plate at -27°C and -40°C is >100 J.
A manufacturing method for directly producing heavy-thickness rack steel plates using continuous casting slabs. Raw materials are formulated according to the chemical composition of the heavy-thickness rack steel plate, and the process sequentially includes KR hot metal pretreatment, converter smelting, LF refining, RH refining, and continuous casting to produce high-purity molten steel and continuous casting slabs with a thickness of 370 mm or above, exhibiting low center segregation and porosity. Compared to the invention with publication number CN102345045A, which uses VD refining and ingot casting, the method described in "Direct Production of Heavy-Thickness Rack Steel Plates Using Continuous Casting Slabs and Their Manufacturing Method" employs RH refining and continuous casting. RH refining enables the production of molten steel with lower hydrogen content to ensure the anti-hydrogen-induced cracking capability and core properties of the rack steel plate. The core quality of slabs produced by continuous casting (e.g., center segregation and porosity) is superior to that of ingots produced by ingot casting, which is beneficial for ensuring the core properties of the rack steel plate.
After continuous casting, the slabs are covered and slowly cooled to further reduce hydrogen content, thereby preventing hydrogen-induced cracking and ensuring core properties. After slow cooling, the slab surfaces are cleaned while warm to ensure surface quality and prevent crack formation during flame cleaning.

The processed continuous casting slabs are heated to 1,180–1,280°C and held for 2–3 hours to fully dissolve alloy elements in the steel, enabling their strengthening and toughening effects and ensuring uniformity in the composition and properties of the final product. After holding and high-pressure water descaling, the slabs undergo two-stage rolling. The first stage (rough rolling) starts at 1,050–1,150°C with a total reduction of 40%, employing heavy reduction rolling. Compared to the conventional maximum reduction rate of approximately 10% per pass in rough rolling for heavy-thickness steel plates, the method requires a reduction rate of 15% per pass to ensure full healing of core defects in the continuous casting slabs, thereby guaranteeing the core properties of the heavy-thickness rack steel plate. The second stage (finish rolling) starts at 870–930°C with a total reduction of 30%. After rolling, the plates are air-cooled and straightened.
The straightened plates are air-cooled on the cooling bed to the maximum temperature suitable for handling, followed by pile slow cooling (48 hours) or controlled slow cooling (held at 550–650°C for 24–72 hours and then slowly cooled) to sufficiently reduce or eliminate hydrogen in the rolled plates, ensuring the core properties of the finished steel plates.
The plates, cooled to room temperature, undergo quenching and tempering treatment to obtain the finished rack steel plates. The quenching heating process is conducted in a continuous furnace to precisely control the heating temperature and time: quenching heating temperature is 900–930°C, in-furnace time is 1.8–2.0 minutes per millimeter, followed by water quenching in a quenching machine. Tempering treatment must also be performed in a continuous furnace to precisely control the heating temperature and time: tempering temperature is 600–660°C, in-furnace time is 2.8–4.0 minutes per millimeter, after which the plates are air-cooled to room temperature.