How the Grade Is Named
08Ni3DR is a steel plate for low-temperature pressure vessels, used to manufacture equipment such as liquefied natural gas storage tanks and the containment tanks of LNG carriers. The designation is descriptive. The 08 refers to a nominal carbon content of 0.08 percent. Ni3 refers to a nominal nickel content of 3 percent, with the actual content controlled in the range of 3.25 to 3.70 percent. R identifies a pressure vessel application, and the grade belongs to the low-temperature pressure vessel steel family with an impact test temperature of -100 C.
The nickel addition is what makes the grade suitable for cryogenic service. Nickel improves the low-temperature toughness of ferritic steel, so the plate resists brittle fracture at -100 C while retaining a strength level that satisfies pressure vessel design rules. This places the grade between the conventional -40 C and -70 C low-temperature steels and the higher nickel grades used at -196 C.
Delivery Condition
Plate is delivered in one of the following conditions, as stated in the order:
Normalized, with accelerated cooling permitted, followed by tempering.
Off-line quenching followed by tempering, where a higher strength level is required.
Normalized delivery for plate of not more than 25 mm thickness, when the order permits.
The tempering temperature is not less than 620 C. The delivery condition can also be specified according to the technical requirements of the project, which allows the user to match the heat treatment to the design strength and toughness values.
Chemical Composition and Mechanical Properties
| Item | Requirement |
|---|---|
| Carbon | 0.08 percent nominal |
| Nickel | 3.25-3.70 percent |
| Minimum yield strength | 320 MPa |
| Tensile strength | 490-620 MPa |
| Minimum elongation | 20 percent |
| Impact test temperature | -100 C |
| Minimum tempering temperature | 620 C |
Charpy V-notch impact testing at -100 C is a mandatory requirement for the grade. The minimum absorbed energy is agreed at the time of order, and higher energy levels are specified for critical containment components. Phosphorus and sulphur are restricted because both reduce the toughness of the plate and of the heat affected zone after welding.
Applications
Liquefied natural gas storage tanks and LNG carrier containment tanks
Ball tanks and spherical storage vessels
Reactors and reactor internals
Heat exchangers and separators
Pressure shells for nuclear power equipment
Boiler drums, pipelines and turbine volutes
Petrochemical and power station equipment operating at low temperature
Fabrication and Welding
The plate is welded with consumables matched to the strength level and the service temperature, and the procedure is qualified with impact testing at -100 C. Heat input and interpass temperature are controlled within the qualified range, and preheat is used as required for the thickness and the carbon equivalent of the actual heat. Because the grade depends on its tempered structure, any post-weld heat treatment is applied at a temperature consistent with the tempering temperature of the base plate.
Cutting is done by plasma or mechanical shearing, edges are dressed, and cold forming is carried out with adequate bend radii. Where hot forming is used, a subsequent heat treatment restores the specified properties. Cleanliness and the avoidance of surface damage matter throughout, because surface defects act as stress raisers in low-temperature service.
Inspection and Certificates
Each plate is delivered with a certificate stating the heat number, chemical analysis, tensile results, impact results at -100 C, delivery condition and any supplementary test results. Ultrasonic examination can be ordered to verify internal soundness, and dimensional inspection covers thickness, flatness, length, width and edge condition. Traceability from the heat number to the certificate is maintained so that the fabricator can document the material for the pressure vessel file.
Frequently Asked Questions
Q: What does 08Ni3DR mean?
A: 08 indicates a nominal carbon content of 0.08 percent, Ni3 indicates a nominal nickel content of 3 percent, D and R indicate a low-temperature pressure vessel application, and the grade is impact tested at -100 C.
Q: What is the actual nickel content of the plate?
A: The nominal content is 3 percent and the actual content is controlled in the range of 3.25 to 3.70 percent.
Q: How is 08Ni3DR delivered?
A: Normalized with accelerated cooling permitted plus tempering, or off-line quenched plus tempered, with strip of not more than 25 mm thickness possibly supplied normalized when the order allows.
Q: What is the minimum tempering temperature?
A: Not less than 620 C.
Q: What is the minimum yield strength?
A: 320 MPa, with tensile strength in the 490 MPa to 620 MPa range and a minimum elongation of 20 percent.
Q: Where is the grade mainly used?
A: In liquefied natural gas storage tanks, LNG carrier containment tanks, ball tanks, reactors, heat exchangers and similar low-temperature pressure equipment.