SM400 Steel Plate: SM400A, SM400B and SM400C to JIS G3106

Dec 04, 2025 Leave a message

SM400 is a rolled steel for welded structures defined by the Japanese Industrial Standard JIS G3106. The designation decodes simply: S for steel, M for welding structure, and 400 for the 400 MPa class minimum tensile strength. Three grades are covered, SM400A, SM400B and SM400C, and all three share the same strength level while differing in chemical limits and in the impact test temperature they must satisfy.

Grade Definition and Impact Requirement

Grade Impact test Typical plate thickness range
SM400A Not required Up to 200 mm, thickness dependent limits
SM400B Charpy V-notch at 20 C Specified to about 100 mm
SM400C Charpy V-notch at 0 C Specified to about 100 mm

The letter suffix therefore describes toughness, not strength. A buyer who needs guaranteed notch toughness at sub-zero or even at ambient service temperature has to specify SM400B or SM400C, because SM400A carries no impact requirement under JIS G3106 at all.

Chemical Composition to JIS G3106, Ladle Analysis

Grade Thickness C max Si max Mn P max S max
SM400A 50 mm and under 0.23 % Not specified 2.5 x C minimum 0.035 % 0.035 %
SM400A Over 50 mm 0.25 % Not specified 2.5 x C minimum 0.035 % 0.035 %
SM400B 50 mm and under 0.20 % 0.35 % 0.60-1.50 % 0.035 % 0.035 %
SM400B Over 50 mm 0.22 % 0.35 % 0.60-1.50 % 0.035 % 0.035 %
SM400C Up to 100 mm 0.18 % 0.35 % 0.60-1.50 % 0.035 % 0.035 %

Two points deserve attention because they are frequently misread in supplier literature. First, SM400A does not have an absolute manganese range: the minimum is defined as 2.5 times the actual carbon content, so manganese and carbon have to be considered together. Second, silicon is not a specified element for SM400A, yet it is capped at 0.35 % for SM400B and SM400C, which is one reason the B and C grades are preferred for welding critical structures.

Mechanical Properties

Yield strength falls as plate thickness rises, while the tensile range stays constant at 400-510 MPa for all three grades. The table below reproduces that thickness dependence, which is the single most important input when checking a design against the standard.

Grade Yield min, 16 mm and under 16-40 mm 40-75 mm 75-100 mm 100-160 mm 160-200 mm Tensile strength
SM400A 245 MPa 235 MPa 215 MPa 215 MPa 205 MPa 195 MPa 400-510 MPa
SM400B 245 MPa 235 MPa 215 MPa 215 MPa 205 MPa Not specified 400-510 MPa
SM400C 245 MPa 235 MPa 215 MPa 215 MPa Not specified Not specified 400-510 MPa

Because the tensile range is identical for the three grades, a mill certificate showing 400-510 MPa does not by itself prove which grade was supplied. Chemical composition and the impact test record are what distinguish SM400A, SM400B and SM400C in practice, so both items should be requested on the inspection document.

Weldability and Fabrication Notes

Carbon content is held at or below 0.23 %, and at 0.18 % for SM400C, which keeps carbon equivalent and hardness in the heat-affected zone low.

For thin and medium plate welded with conventional processes, preheat is not normally mandatory, although moisture control on the joint faces still matters.

Thicker sections, high restraint joints and low ambient temperature increase cracking risk and should be assessed with a hydrogen-aware procedure, as described for ferritic steels in EN 1011-2.

SM400 responds well to all common arc processes, including shielded metal arc, gas metal arc, submerged arc and flux-cored welding.

Applications and Selection Notes

SM400 is used for building frames, bridge components, ship hull structures, storage tanks and general welded fabrications where a 400 MPa tensile class steel with reliable weldability is sufficient. It is cold formable and readily machined, which suits it to fabrication shops that cut, drill and bend plate before assembly.

One recurring misunderstanding is worth correcting: SM400 is sometimes marketed as a high-strength plate. It is not. Its minimum yield strength of 195-245 MPa depending on thickness places it in the general structural steel range, well below the 460 MPa and 690 MPa classes. Buyers who need higher strength should look at the SM490 series to JIS G3106 or the quenched and tempered grades to EN 10025-6 instead.

Frequently Asked Questions

Q: What is the difference between SM400A, SM400B and SM400C?
The difference is chemical control and impact testing, not strength. SM400A has no impact requirement, SM400B is impact tested at 20 C, and SM400C is impact tested at 0 C with a tighter carbon limit.

Q: Which standard covers SM400 steel plate?
SM400A, SM400B and SM400C are defined by JIS G3106, the Japanese standard for rolled steels for welded structures.

Q: What does the 400 in SM400 mean?
It refers to the 400 MPa class minimum tensile strength. The guaranteed tensile range is 400-510 MPa for all three grades regardless of thickness.

Q: Is SM400 a high-strength steel?
No. SM400 is a general structural steel of the 400 MPa tensile class with a minimum yield strength between 195 MPa and 245 MPa depending on thickness, so it sits below the SM490 and 690 MPa classes.

Q: Does SM400 need preheating before welding?
For thin and medium plate under normal shop conditions preheat is usually not required, but thick sections, high restraint and cold ambient conditions should be evaluated with a qualified welding procedure that accounts for hydrogen.

Q: Why does yield strength differ with thickness?
JIS G3106 sets lower minimum yield values as plate thickness increases, because rolling reduction and cooling rate change through the section. Design calculations must use the value that corresponds to the actual thickness ordered.