SA204 Grade C in the ASME Pressure Vessel System
SA204 Grade C is a molybdenum-alloy steel plate specification issued in ASME SA204/SA204M for welded pressure vessels intended for high temperature service. The A204 series contains Grades A, B and C, which share the same molybdenum range and differ mainly in carbon content, so Grade C is the highest strength of the three and is specified where the design needs a stronger plate without moving to a low alloy chromium-molybdenum grade.
The molybdenum addition is the key to the grade. It raises the elevated temperature strength of the steel compared with plain carbon plate and improves resistance to hydrogen attack in refinery and petrochemical service, while the carbon level gives a tensile range that can be matched by the weld procedure.
Chemical Composition by Thickness
Carbon content is allowed to rise as the plate becomes thicker, because heavier sections cool more slowly during rolling and normalizing and therefore need more carbon to reach the specified strength.
| Element | T ≤ 25 mm | 25 < T ≤ 50 mm | 50 < T ≤ 100 mm | T > 100 mm |
|---|---|---|---|---|
| C, max | 0.23 | 0.26 | 0.28 | 0.28 |
| Si | 0.15-0.40 | |||
| Mn, max | 0.90 | |||
| P, max | 0.035 | |||
| S, max | 0.035 | |||
| Mo | 0.45-0.60 | |||
Sulphur and phosphorus are held at the same low levels at every thickness, which matters because these residual elements drive both temper embrittlement and loss of notch toughness in thick sections.
Mechanical Properties and High Temperature Behaviour
| Property | Requirement |
|---|---|
| Minimum yield strength Re | 295 MPa |
| Tensile strength Rm | 515-655 MPa |
| Minimum elongation in 50 mm (2 in) | 20 % |
| Minimum elongation in 200 mm (8 in) | 16 % |
| Rolling type | Boiler and pressure vessel steel plate |
| Standard | ASME SA204/SA204M |
Because the grade is intended for hot duty, the design check does not stop at room temperature properties. Allowable stresses at elevated temperature are taken from the design stress tables of ASME BPVC Section II Part D for the specified material, and the plate is qualified by tensile testing supplemented, where the design demands it, by elevated temperature tensile or creep related data agreed with the purchaser.
Delivery Condition, Heat Treatment and Testing
Delivery conditions: as rolled, normalized, or normalized and stress relieved, according to thickness and to the requirements of the construction code.
Thick sections are normally supplied normalized so that the carbon and molybdenum combination produces a uniform ferrite-pearlite microstructure.
Plates may be supplied with post-weld heat treatment simulation if the vessel will be stress relieved after fabrication, so that the purchaser sees properties in the heat treated condition.
Mechanical testing is carried out on samples taken in accordance with ASME SA-20/SA-20M general requirements, covering tensile, elongation and impact properties as specified on the order.
Inspection documents are issued as material test certificates with chemical analysis, heat number and mechanical results traceable to each plate.
Fabrication, Welding and Applications
SA204 Grade C is readily formed, machined and welded in the normalized condition. Welding is performed with low hydrogen consumables under a procedure qualified to ASME BPVC Section IX, with preheat and interpass control chosen according to thickness, restraint and the carbon content of the plate. Because the carbon level rises with thickness, thick plate benefits from a slightly higher preheat and from careful control of heat input, and post-weld heat treatment is applied where the construction code requires it for the finished wall thickness.
Reactors, heat exchanger shells and channel sections
Separators, drums and spherical storage tanks
Liquefied petroleum gas and liquefied gas storage equipment
Boiler steam drums, headers and high pressure piping in power stations
Petrochemical and refinery pressure equipment operating at elevated temperature
Frequently Asked Questions
Q: What is SA204 Grade C made of?
It is a carbon-molybdenum steel plate with 0.45-0.60 % molybdenum, carbon controlled between 0.23 and 0.28 % depending on thickness, and maximum sulphur and phosphorus of 0.035 % each.
Q: How does Grade C differ from Grades A and B?
The three grades share the same molybdenum range and differ mainly in carbon content, which raises the specified strength from Grade A through Grade C.
Q: What strength does SA204 Grade C provide?
A minimum yield strength of 295 MPa and a tensile range of 515-655 MPa, with a minimum elongation of 20 % in a 50 mm gauge length.
Q: Why is molybdenum added to this steel?
Molybdenum improves strength retention at elevated temperature and resistance to hydrogen attack, which is why the grade is used in refinery, petrochemical and power station pressure equipment.
Q: Which thicknesses are available?
The grade is supplied from 6 mm to 150 mm as standard, with heavier plates up to about 300 mm produced to agreement, and widths and lengths agreed from the mill range for the ordered thickness.
Q: Is post-weld heat treatment required?
Where the construction code requires stress relief for the finished wall thickness it is applied, and plates can be ordered with post-weld heat treatment simulation so that the delivered properties represent the heat treated condition.