Why S690Q Welding Needs a Controlled Procedure
S690Q is a quenched and tempered structural steel plate supplied under EN 10025-6, with a European material number of 1.8931 and a minimum yield strength of 690 MPa at thicknesses from 8 mm to 50 mm. Its strength comes from a martensitic or bainitic microstructure produced by quenching followed by tempering. That microstructure is the reason the material performs so well in service and also the reason welding is the critical step in fabrication: excessive heat input, poor hydrogen control or an incorrect tempering cycle can locally destroy the properties that the plate was bought for.
This guide sets out a practical welding sequence for S690Q plate, covering preparation, consumable selection, thermal control, post-weld treatment and inspection. It is written for workshop and project engineers who must translate the standard into a workable welding procedure specification.
Base Material Data to Confirm Before Welding
EN 10025-6 limits the chemical composition of S690Q as follows, in maximum percentages by mass.
| C | Si | Mn | P | S | N | B | Cr | Cu | Mo | Nb | Ni | V | Ti |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 0.20 | 0.80 | 1.70 | 0.025 | 0.015 | 0.015 | 0.005 | 1.50 | 0.50 | 0.70 | 0.06 | 2.00 | 0.12 | 0.05 |
The alloying system is a low-carbon, micro-alloyed one: boron and nickel raise hardenability, while niobium, vanadium and titanium form carbonitrides that refine the tempered structure. Low carbon keeps the carbon equivalent moderate for a steel of this strength, which is what makes controlled welding possible at all.
Mechanical properties of S690Q and its low-temperature variant S690QL follow the thickness of the plate.
| Grade | Thickness (mm) | ReH min (MPa) | Rm (MPa) | Elongation min (%) | Charpy min |
|---|---|---|---|---|---|
| S690Q | 8 to 50 | 690 | 770–940 | 14 | 30 J at −20 °C |
| S690QL | 8 to 50 | 690 | 770–940 | 14 | 30 J at −40 °C |
Note that the grade letter Q always means quenched and tempered delivery; the L suffix adds low-temperature impact performance. Both variants must never be flame-straightened or hot-formed in the same way as ordinary carbon steel.
Pre-Welding Preparation
Groove preparation and cleaning
Prepare the groove mechanically, by milling or plasma cutting, rather than by flame cutting. Flame cutting hardens the cut face and can leave a brittle layer that acts as a crack initiation site in a 690 MPa steel.
Remove oil, grease, rust, scale, paint and moisture within at least 20 mm on both sides of the groove.
Keep the joint dry. Hydrogen is the main cause of delayed cracking in quenched and tempered steels, and moisture on the plate surface is a direct hydrogen source.
Check fit-up carefully; excessive root gaps force the welder to use higher current, which pushes heat input beyond the qualified range.
Preheating
Preheating temperature increases with plate thickness and is applied by electrical resistance heaters so that the whole joint area reaches a uniform temperature.
| Plate thickness (mm) | Preheat temperature (°C) |
|---|---|
| Below 16 | 80–120 |
| 16 to 40 | 120–150 |
| Above 40 | 150–200 |
Measure the temperature on the plate face close to the groove, on the opposite side of the joint, and again after any interruption of welding.
Consumables and Welding Parameters
Filler metals must be matched to a 690 MPa base metal rather than to a mild steel. Low-hydrogen flux-cored wires such as E81T1-K2C or basic coated electrodes such as E11018-G are typical choices, with a deposited yield strength of at least 690 MPa and impact energy of 47 J or more at −20 °C.
| Process | Key parameters |
|---|---|
| Submerged arc welding (SAW) | Current 500–600 A, voltage 30–34 V, travel speed 30–40 cm/min, neutral basic flux |
| Gas metal arc welding (GMAW) | 80 % argon with 20 % CO2 shielding gas, current 220–280 A, voltage 28–32 V |
| Interpass temperature | Maximum 200 °C; stop welding and allow cooling before continuing |
| Pass thickness | Maximum about 5 mm per pass, multi-pass sequence for thick plate |
Interpass temperature is the parameter most often ignored in production. Above 200 °C the tempering effect of successive passes accumulates, grains coarsen in the heat-affected zone and toughness falls sharply even though the joint still looks sound.
Use symmetrical welding and back-step (reverse) sequences to balance shrinkage and lower residual stress.
Prefer mechanised or automated processes; manual metal arc welding adds operator variability precisely where consistency matters most.
Tack welds count as part of the joint. They should be made with the same preheat and consumable as the main weld, and defective tacks must be removed rather than buried.
Keep heat input inside the range qualified in the welding procedure qualification record, and record energy input for each run on thick joints.
Post-Weld Heat Treatment and Inspection
Tempering after welding restores toughness in the heat-affected zone and relieves residual stress. S690Q joints are typically tempered at 550–600 °C, with holding time calculated at about one hour per 25 mm of plate thickness, followed by slow cooling in still air or under insulation.
Inspection is carried out at least 24 hours after welding, because hydrogen-assisted cracking in high-strength steel needs time to appear.
| Item | Requirement |
|---|---|
| Ultrasonic testing | Technique to EN ISO 17640, acceptance level 2 of EN ISO 11666 |
| Magnetic particle testing | Technique to EN ISO 17638, acceptance level 2 of EN ISO 23278 |
| Weld tensile / yield strength | Minimum 650 MPa in the transverse tensile test when required by the specification |
| Weld impact energy | 40 J or more at −20 °C in the heat-affected zone and weld metal |
| Hardness survey | Carried out on procedure qualification to confirm that the heat-affected zone hardness stays within the agreed limit |
Troubleshooting Common Weld Defects
Hydrogen-induced cold cracking: remove the cracked region together with surrounding metal to at least twice the crack depth, re-preheat, re-weld and lengthen the post-weld tempering hold.
Hot cracking or solidification cracking: reduce heat input, control the weld bead shape, and select consumables with lower sulphur and phosphorus content.
Loss of joint strength: check that penetration reaches at least 70 % of plate thickness, verify the tempering temperature actually reached, and confirm that no unqualified heat input was used.
Softening in the heat-affected zone: occurs when too many passes are deposited without interpass control; re-qualify the procedure with a measured interpass limit and a maximum heat input.
Welded with the sequence above, an S690Q joint reaches properties that track the base plate closely enough for demanding structures, which is why the grade is common in mobile cranes, mining and earthmoving machinery, heavy vehicle frames, pressure equipment support structures and other applications where weight saving pays for careful fabrication.
Frequently Asked Questions
Q: What is S690Q steel?
S690Q is a quenched and tempered structural steel plate under EN 10025-6 with a European material number of 1.8931 and a minimum yield strength of 690 MPa for thickness from 8 mm to 50 mm.
Q: Why is flame cutting not recommended before welding S690Q?
Flame cutting creates a hardened, locally brittle cut face in high-strength quenched and tempered steel. Mechanical grooving by milling or plasma cutting avoids that layer and reduces cracking risk.
Q: What preheat temperature is used for S690Q plate?
Roughly 80–120 °C below 16 mm thickness, 120–150 °C from 16 to 40 mm, and 150–200 °C above 40 mm, always confirmed by the qualified welding procedure.
Q: What is the maximum interpass temperature?
200 °C. Welding should be stopped when the joint reaches that temperature and resumed only after it has cooled back into the qualified range.
Q: Is post-weld heat treatment always required?
Stress-relief tempering at 550–600 °C is specified for most S690Q fabrication, especially thick and highly restrained joints, because it restores heat-affected zone toughness and removes residual stress.
Q: How soon after welding can inspection be carried out?
Non-destructive testing is normally performed at least 24 hours after completion of welding so that delayed hydrogen cracking has time to develop and be detected.