DNV F36 steel plate,also named as DNV Grade FH36 marine steel plate which have to be done low temperature impacting test under minus 60 centigree and done normalized or TMCP heat treatment for any thickness.
Steel Standard:DNV (Det Norske Veritas)
Rolling Type:Shipbuilding steel plate,High tension ship plate
Thickness:3mm-250mm
Width:1200mm-4200mm
Length:3000mm-18000mm
Heat Treatment:TMCP/Normalized
Chemical Composition
|
DNV F36 high Strength Chemical Composition |
|||||||
|
Grade |
The Element Max (%) |
||||||
|
C |
Si |
Mn |
P |
S |
Al |
N |
|
|
DNV F36 |
0.16 |
0.10-0.50 |
0.9-1.6 |
0.025 |
0.025 |
0.015-0.08 |
0.009 |
|
Nb |
V |
Ti |
Cu |
Cr |
Ni |
Mo |
|
|
0.02-0.05 |
0.05-0.10 |
0.02 |
0.35 |
0.20 |
0.80 |
0.08 |
|
Mechanical Property
|
DNV F36 high general strength property |
|||||||
|
Grade |
|
Mechanical Property |
Charpy V Impact Test |
||||
|
Thickness |
Yield |
Tensile |
Elongation |
Degree |
Energy 1 |
Energy 2 |
|
|
DNV F36 |
mm |
Min Mpa |
Mpa |
Min % |
-60 |
J |
J |
|
t≤50 |
355 |
490-620 |
21% |
24 |
34 |
||
|
50<t≤70 |
355 |
490-620 |
21% |
27 |
41 |
||
|
70<t≤150 |
355 |
490-620 |
21% |
34 |
50 |
||
|
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
|||||||