Alloy 625 is known for superior corrosion resistance in Marine Applications compared to the Alloy 825. Check Difference Between Inconel and Incoloy which is important to know before installation in Sea water and High Temperature Applications.
| Alloy 825 | Alloy 625 | |
|---|---|---|
| Material | nickel-iron-chromium alloy 825 | nickel-chromium alloy 625 |
| Equivalent | W.Nr. 2.4858 UNS N08825 |
W.Nr. 2.4856 UNS N06625 |
| Density | 0.294 lb/cu in | 0.305 lb/cu in |
| Melting Range | 1370-1400°C | 1290-1350°C |
| Curie Temperature | <-196°C | -196°C |
| Thermal Conductivity | 76.8 Btu • in/ft2•h•°F 11.1 W/m •°C. |
68 Btu • in/ft2•h•°F 9.8 W/m •°C. |
Inconel vs Incoloy Chemical Composition
| Incoloy 825 | Inconel 600 | Inconel 625 | Inconel 718 | Inconel 601 | Inconel X750 | Inconel 617 | Inconel 690 | |
|---|---|---|---|---|---|---|---|---|
| C | ≤0.05 | ≤0.15 | ≤0.08 | ≤0.08 | ≤0.1 | ≤0.08 | 0.05-0.15 | ≤0.05 |
| Mn | ≤1 | ≤1 | ≤0.35 | ≤0.35 | ≤1.5 | ≤1 | ≤0.5 | ≤0.5 |
| Fe | ≥22 | 6-10 | rest | rest | rest | 5-9 | ≤3 | 7-11 |
| P | - | ≤0.015 | - | - | ≤0.02 | - | ≤0.015 | - |
| S | ≤0.03 | ≤0.015 | ≤0.015 | ≤0.01 | ≤0.015 | ≤0.01 | ≤0.015 | ≤0.015 |
| Si | ≤0.5 | ≤0.5 | ≤0.35 | ≤0.35 | ≤0.5 | ≤0.5 | ≤0.5 | ≤0.5 |
| Cu | 1.5-3 | ≤0.5 | ≤0.3 | ≤0.3 | ≤1 | ≤0.5 | - | ≤0.5 |
| Ni | 38-46 | ≥72 | 50-55 | 50-55 | 58-63 | ≥70 | ≥44.5 | ≥58 |
| Co | - | - | ≤10 | ≤1 | - | ≤1 | 10-15 | - |
| Al | ≤0.2 | - | ≤0.8 | 0.2-0.8 | 1-1.7 | 0.4-1 | 0.8-1.5 | - |
| Ti | 0.6-1.2 | - | ≤1.15 | - | - | 2.25-2.75 | ≤0.6 | - |
| Cr | 19.5-23.5 | 14-17 | 17-21 | 17-21 | 21-25 | 14-17 | 20-24 | 27-31 |
| Nb+Ta | - | - | 4.75-5.5 | 4.75-5.5 | - | 0.7-1.2 | - | - |
| Mo | 2.5-3.5 | - | 2.8-3.3 | 2.8-3.3 | - | - | 8-10 | - |
| B | - | - | - | - | - | - | ≤0.006 | - |
Tensile and Yield Strength Difference Between Inconel 625 and 825
| Alloy 825 (Ksi (MPa)) |
Alloy 625 (Ksi (MPa)) |
|
|---|---|---|
| Annealed Tubing | 112 (772) | 120-140 (827-965) |
| Annealed Bar | 100 (690) | 120-150 (827-1034) |
| Annealed Plate | 96 (662) | 120-150 (827-1034) |
| Annealed Sheet | 110 (758) | 120-150 (827-1034) |
Alloy 825 vs Alloy 625 Applications and Uses
Inconel Alloy 625
- Engine Exhaust Systems
- Sea-water Applications
- Aircraft Ducting Systems
- Thrust-reverser Systems
- Distillation Columns
- Heat-exchanger And Boilers
- Seals
- Springs
- Bellows
Incoloy Alloy 825
- Chemical Processing
- Acid Production
- Nuclear Fuel Reprocessing
- Oil And Gas Recovery
- Pickling Operations
Charpy Impact Strength of Inconel 625 vs 825 Plates
Inconel Alloy 625
| Temperature | Orientation | Inconel Impact Strength | |
|---|---|---|---|
| J | ft-lb | ||
| 29°C | Longitudinal | 65, 66, 68 | 48, 49, 50 |
| Transverse | 62, 66, 70 | 46, 49, 51.5 | |
| -79°C | Longitudinal | 53, 57, 60 | 39, 44, 49 |
| Transverse | 53, 57, 60 | 39, 42, 44 | |
| -196°C | Longitudinal | 47, 47, 48 | 35, 35, 35.5 |
| Transverse | 42, 43, 49 | 31, 32, 36 | |
Incoloy Alloy 825
| Temperature | Orientation | Incoloy Impact Strength | |
|---|---|---|---|
| J | ft-lb | ||
| Room | Longitudinal | 107 | 79.0 |
| Transverse | 113 | 83.0 | |
| -43 °C | Longitudinal | 106 | 78.0 |
| Transverse | 106 | 78.5 | |
| -196 °C | Longitudinal | 91 | 67.0 |
| Transverse | 97 | 71.5 | |
| -253 °C | Longitudinal | 92 | 68.0 |
| Transverse | 92 | 68.0 | |
Email: alloy@gneesteelgroup.com
Whatsapp (WeChat): +86-15824687445
FAQ
Q: What is the ASTM standard for Inconel 625?
A: Inconel 625 Welded Pipes are a superalloy that has been solid solution strengthened for use in both elevated temperature and high pressured applications. The pipes produced under ASTM B444 UNS N06625 specification often indicates that these pipes have a seamless construction.
Q: What is the grade of N06625 material?
A: INCONEL nickel-chromium alloy 625 (UNS N06625/W.Nr. 2.4856) is used for its high strength, excellent fabricability (including joining), and outstanding corrosion resistance. Service temperatures range from cryogenic to 1800°F (982°C).
Q: What material is ASTM B444 uns N06625?
A: Inconel alloy 625
The alloy 625 tubes, which are widely used for superheater or heat exchanger tubing, are generally manufactured as per ASTM B444 (ASME SB-444) UNS N06625. It is a typical nickel-chromium-molybdenum-columbium alloy, which is commercially known as a proprietary brand of "Inconel alloy 625".
Q: What is the difference between N08825 and N06625?
A: Inconel 625 VS Incoloy 825 (UNS N06625 VS UNS N08825)
The major difference between two materials is the nickel content value, for Inconel 625 Nickel 58% minimum, and for Incoloy 825 Nickel at range of 38% to 46%. And this makes the 625 material more expensive.
Q: What is the difference between Inconel 825 and SS316?
A: Incoloy 825 vs SS316 - What's the Difference
Incoloy 825 is ideal for aggressive and highly corrosive environments, high-temperature applications, or resistance to stress corrosion cracking is essential. On the other hand, SS316 is ideal for applications requiring good resistance to general corrosion and pitting corrosion.
Q: What is the difference between Grade 1 and Grade 2 alloy 625?
A: Grade 1 is typically annealed around 1600F to 1800F (about 871°C to 982°C) to provide good ductility and corrosion resistance while maintaining higher strength than Grade 2. Grade 2 is heat-treated above 2000F (about 1093°C), which enhances creep and stress rupture resistance while retaining corrosion resistance.
| Other steel plate | ||||
| Name | Material | Specification (mm) | Tons | Remark |
| Low Alloy | Q345A, Q345B, Q345C, Q345D, Q345E, Q390, Q420, Q460C, ST52-3, S355J2+N, SS400, SA302GrC, S275NL, 35CrMo | 6 - 350 | 5788.56 | Normalizing, tempered ,controlled rolling, hot rolling , Hot rolling,1st inspection, 2nd inspection, 3rd inspection |
| Pressure Vessel Plate | Q245R, Q345R, Q370R, 16MnDR, 09MnNiDR, 15CrMoR, 14Cr1MoR, 12Cr2Mo1R, SA516Gr60, SA516Gr70, SA516Gr485, SA285, SA387Gr11, SA387Gr12, SA387Gr22, P265,P295,P355GH,Q245R(R-HIC),Q345R(R-HIC) | 3 - 300 | 8650 | Normalizing, tempered ,controlled rolling, hot rolling , Hot rolling,1st inspection, 2nd inspection, 3rd inspection |
| High-Strength Plate | WH785D/E,Q960D/E, Q890D/E,WH60D/E,WH70B,Q550D,Q590D,Q690D/E | 8 - 120 | 3086.352 | Quenched and tempered |
| Wear-Resistant Plate | NM360, NM400, NM450, NM500 | 6 - 150 | 3866.297 | Quenched and tempered |
| Bridge Plate | Q235qC, Q345qC, Q370qC, Q420qC, Q345qDNH, Q370qDNH, A709 - 50F - 2, A709 - 50T - 2 | 8 - 200 | 2853.621 | Hot rolling, normalized ,hot rolling controlled rolling, quenched and tempered + toughness and brittleness |