LR AH40 is a high-strength shipbuilding steel plate certified by Lloyd's Register (LR). The "A" grade signifies it is impact tested at 0°C, ensuring reliable toughness for general marine environments . It has a minimum yield strength of 390 MPa and tensile strength ranging from 510 to 650 MPa, with a minimum elongation of 20% . The chemical composition is strictly controlled with carbon ≤0.18% and manganese 0.90-1.60% . This grade is widely used for hull structures, decks, and offshore platforms requiring an excellent balance of strength and weldability .
LR AH62 is an ultra-high-strength marine steel plate also certified by Lloyd's Register (LR), designed for demanding structural applications. It is impact tested at 0°C and has a minimum yield strength of 440 MPa and tensile strength ranging from 620 to 800 MPa, with a minimum elongation of 19% . The chemical composition is more complex than AH40, featuring carbon ≤0.21%, manganese ≤1.70%, and additional alloying elements including nickel (0.70-1.80%), chromium (0.40-1.60%), and molybdenum (≤0.70%) to achieve superior mechanical properties . This grade is delivered in normalized or quenched and tempered (QT) conditions and is used for critical components in large vessels and offshore structures requiring maximum strength-to-weight ratio .
Both LR AH40 and LR AH62 are LR-certified high-strength marine steels with impact toughness tested at 0°C, ensuring reliable performance in general marine environments. Their primary difference lies in strength level: AH40 offers a minimum yield strength of 390 MPa with tensile strength of 510-650 MPa, suitable for general high-strength hull construction and offshore platforms, while AH62 provides a substantially higher minimum yield strength of 440 MPa with tensile strength reaching 620-800 MPa, designed for more demanding load-bearing applications requiring superior strength-to-weight ratio . Both grades feature controlled chemical composition and maintain good weldability for critical marine service, though AH62 requires more complex alloying and advanced processing like quenching and tempering to achieve its enhanced mechanical properties .
Chemical Composition
|
LR AH40 high Strength Chemical Composition |
|||||||
|
Grade |
The Element Max (%) |
||||||
|
C |
Si |
Mn |
P |
S |
Al |
N |
|
|
LR AH40 |
0.18 |
0.05 |
0.9-1.6 |
0.035 |
0.035 |
0.015 |
|
|
Nb |
V |
Ti |
Cu |
Cr |
Ni |
Mo |
|
|
0.02-0.05 |
0.03-0.10 |
0.02 |
0.35 |
0.20 |
0.40 |
0.08 |
|
|
LR AH62 extra high Strength Chemical Composition |
|||||||
|
Grade |
The Element Max (%) |
||||||
|
C |
Si |
Mn |
P |
S |
Al |
N |
|
|
LR AH62 |
0.21 |
0.55 |
1.70 |
0.035 |
0.035 |
0.015 |
0.020 |
|
Nb |
V |
Ti |
Cu |
Cr |
Ni |
Mo |
|
|
0.02-0.05 |
0.03-0.10 |
0.02 |
|
|
|
|
|
Mechanical Property
|
LR AH40 high strength property |
|||||||
|
Grade |
|
Mechanical Property |
Charpy V Impact Test |
||||
|
Thickness |
Yield |
Tensile |
Elongation |
Degree |
Energy 1 |
Energy 2 |
|
|
LR AH40 |
mm |
Min Mpa |
Mpa |
Min % |
0 |
J |
J |
|
t≤50 |
390 |
510-650 |
20% |
26 |
39 |
||
|
50<t≤70 |
390 |
510-650 |
20% |
31 |
46 |
||
|
70<t≤100 |
390 |
510-650 |
20% |
37 |
55 |
||
|
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
|||||||
|
LR AH62 extra high strength property |
|||||||
|
Grade |
|
Mechanical Property |
Charpy V Impact Test |
||||
|
Thickness |
Yield |
Tensile |
Elongation |
Degree |
Energy 1 |
Energy 2 |
|
|
LR AH62 |
mm |
Min Mpa |
Mpa |
Min % |
0 |
J |
J |
|
t≤50 |
620 |
720-890 |
17% |
41 |
62 |
||
|
50<t≤70 |
620 |
720-890 |
17% |
41 |
62 |
||
|
70<t≤100 |
620 |
720-890 |
17% |
41 |
62 |
||
|
Note: Energy 1 is transverse impact test, Energy 2 is longitudinal |
|||||||