A517GrQ steel plate thickness 8-150mm cutting and deep processing technical service introduction

Aug 22, 2025 Leave a message

ASTM-A517-A517M-Standard-Specification.pdf

A517GrQ is a high-strength quenched and tempered steel plate, a type of killed steel, with ultra-high strength, uniform and good low-temperature toughness and low crack sensitivity requirements.

A517GrQ steel plate grade indication: "A": indicates American standard alloy steel; "517": indicates that the yield strength of the steel plate is 517Mpa. "Gr": Abbreviation for Grade.

 

A517GrQ High Strength Plate Chemical Composition:

Standards

C

Mn

P

S

Si

Ni

Cr

Mo

V

A517GrQ

0.12-0.23

0.95-1.30

0.025

0.025

0.15-0.35

1.20-1.50

1.0-1.5

0.4-0.6

0.03-0.08

 

A517GrQ Steel Plate Mechanical Properties:

Standards

Tensile strength, Mpa

Yield strength, Mpa

Elongation in 2mm

A517GrQ

725-930

620

14

 

 

wechat2025-07-17160312175

Heat Treatment:

The A517GrQ/A517 Grade Q steel plate undergoes a rigorous heat treatment process to enhance its mechanical properties. The steel is heated to a temperature not lower than 900°C, followed by quenching in water or oil. Subsequently, it is tempered at a temperature not lower than 620°C. This process ensures a homogeneous microstructure and optimal mechanical characteristics.

A517GrQ Steel Plate Production and Cutting Process Flow:

A manufacturing method for direct production of heavy-thickness rack steel plates using continuous casting slabs to produce the heavy-thickness rack steel plate, raw materials are formulated according to its chemical composition. The process sequentially includes KR hot metal pretreatment, converter smelting, LF refining, RH refining, and continuous casting to produce high-purity molten steel and continuous casting slabs with a thickness of 370 mm or above, exhibiting low center segregation and porosity. Compared to the invention disclosed in patent CN102345045A, which uses VD refining and ingot casting, the method described in Direct Production of Heavy-Thickness Rack Steel Plates Using Continuous Casting Slabs and Their Manufacturing Method employs RH refining and continuous casting. RH refining enables the production of molten steel with lower hydrogen content, ensuring the anti-hydrogen-induced cracking capability and core properties of the rack steel plate. The continuous casting method produces slabs with superior core quality (e.g., reduced center segregation and porosity) compared to ingot casting, thereby ensuring the core performance of the rack steel plate.

After continuous casting, the slabs are covered and slowly cooled to further reduce hydrogen content, thus preventing hydrogen-induced cracking and ensuring core properties. Following slow cooling, the slab surfaces are cleaned while warm to ensure surface quality and prevent crack formation during flame cleaning.

 

wechat2025-07-17160357918

The processed continuous casting slabs are heated to 1,180–1,280°C and held for 2–3 hours to fully dissolve alloy elements in the steel, enabling their strengthening and toughening effects and ensuring uniformity in the composition and properties of the final product. After holding and high-pressure water descaling, the slabs undergo two-stage rolling. The first stage (rough rolling) starts at 1,050–1,150°C with a total reduction of 40%, employing heavy reduction rolling. Compared to the conventional maximum reduction rate of approximately 10% per pass in rough rolling for heavy-thickness steel plates, the method described in Direct Production of Heavy-Thickness Rack Steel Plates Using Continuous Casting Slabs and Their Manufacturing Method requires a reduction rate of 15% per pass to ensure full healing of core defects in the continuous casting slabs, thereby guaranteeing the core properties of the heavy-thickness rack steel plate. The second stage (finish rolling) starts at 870–930°C with a total reduction of 30%. After rolling, the plates are air-cooled and straightened.

The straightened plates are air-cooled on the cooling bed to the maximum temperature suitable for handling, followed by pile slow cooling (48 hours) or controlled slow cooling (held at 550–650°C for 24–72 hours and then slowly cooled) to sufficiently reduce or eliminate hydrogen in the rolled plates, ensuring the core properties of the finished steel plates.

The plates, cooled to room temperature, undergo quenching and tempering treatment to obtain the finished rack steel plates. The quenching heating process is conducted in a continuous furnace to precisely control the heating temperature and time: quenching heating temperature is 900–930°C, and in-furnace time is 1.8–2.0 minutes per millimeter, followed by water quenching in a quenching machine. Tempering treatment must also be performed in a continuous furnace to precisely control the heating temperature and time: tempering temperature is 600–660°C, and in-furnace time is 2.8–4.0 minutes per millimeter, after which the plates are air-cooled to room temperature.