9Ni590A 9% Ni Vessel Plate: Standard, Melting and Testing

Feb 19, 2024 Leave a message

Grade Definition, Standard Basis and Melting Route

9Ni590A is a 9% nickel steel plate intended for low-temperature pressure vessels and is produced under GB 24510, the Chinese standard that applies to 9% nickel steel plate with a thickness of not more than 50 mm. The grade delivers excellent low-temperature toughness together with high strength at -196 C, and it is the base material for the containment of liquefied natural gas in tanks and on ships.

The letter A in the grade identifies the specification variant, which is differentiated by the melting route and the supplementary inspection requirements rather than by the basic strength level. Material is ordered by thickness, delivery condition and the supplementary requirements listed in the purchase order, such as ultrasonic testing level.

9Ni590A plate is smelted in an oxygen converter or an electric furnace and then refined outside the furnace. Secondary metallurgy is used to reduce phosphorus, sulphur and gas content, because cleanliness has a direct effect on the low-temperature toughness of the finished plate. Vacuum degassing and careful control of nickel addition are part of the accepted production route, and the low carbon level, generally not more than 0.10 percent, is maintained to limit the formation of brittle phases during quenching.

Chemical Composition and Properties

Item Value
Nickel content 8.50-9.50 percent
Maximum carbon 0.10 percent
Maximum phosphorus 0.015 percent
Maximum sulphur 0.005 percent
Minimum yield strength 590 MPa
Tensile strength 680-820 MPa
Minimum elongation 18 percent
Impact test temperature -196 C

Delivery condition is quenched and tempered, or twice quenched and tempered where a higher toughness level is required. The heat treatment determines the final balance of strength and toughness, and the mechanical tests are taken from plate that has received the complete treatment cycle.

Non-Destructive Testing

Plate is ultrasonic tested sheet by sheet. The testing method and acceptance level are agreed between the supplier and the purchaser at the time of order; where no level is specified, the requirements of JB/T 4730.3, the ultrasonic testing standard for pressure equipment, apply at grade I. Other special requirements can be added to the order by agreement, for example additional surface examination or tighter internal quality levels for thick plate intended for highly stressed containment components.

Applications

Liquefied natural gas storage tanks

Liquefied natural gas carriers and their containment systems

Cryogenic pressure vessels and cold boxes

Liquefied gas storage and transport equipment operating near -196 C

Fabrication and Welding

Welding is carried out with consumables matched to the cryogenic service, and the procedure is qualified with impact testing at -196 C so that the weld metal and the heat affected zone are proven alongside the base plate. Heat input and interpass temperature are controlled in a narrow band, and preheat is generally avoided or limited to a low level consistent with the qualified procedure, because excessive heat slows cooling and can reduce toughness in the heat affected zone.

Cutting is performed by plasma or mechanical shearing followed by edge dressing. Forming is done cold with controlled radii, and any hot forming or post-weld heat treatment is agreed in advance so that the properties verified by the mill are not degraded. Cleanliness during fabrication is important, since the plate surface must remain free from contamination that could affect welding.

Quality Control and Documentation

Each plate is delivered with a certificate showing the heat number, the chemical analysis, the tensile results, the impact results at -196 C, the heat treatment records and the ultrasonic testing report. The certificate allows the fabricator and the end user to trace every plate to its original test data, which is a common requirement for cryogenic equipment projects.

Frequently Asked Questions

Q: What standard covers 9Ni590A plate?

A: GB 24510, which applies to 9% nickel steel plate with a thickness of not more than 50 mm.

Q: How is 9Ni590A steel smelted?

A: In an oxygen converter or electric furnace, followed by secondary refining outside the furnace to control sulphur, phosphorus and gas content.

Q: Is ultrasonic testing mandatory?

A: Plate is ultrasonic tested sheet by sheet. Where the level is not specified in the order, the requirements of JB/T 4730.3 grade I are applied, and other levels can be agreed between supplier and purchaser.

Q: What is the delivery condition?

A: Quenched and tempered, or twice quenched and tempered when the order requires higher toughness.

Q: Where is the grade used?

A: Mainly for liquefied natural gas storage tanks, LNG carriers and other low-temperature pressure vessels operating at about -196 C.

Q: Why is the carbon content kept so low?

A: Low carbon limits the formation of hard, brittle phases during quenching and helps the plate achieve the required toughness at -196 C.