What Is 30CrNiMo8 (1.6580) Steel?
30CrNiMo8 is a chromium-nickel-molybdenum alloy steel defined in EN 10083-3, the European standard for quenched and tempered steels. It is normally supplied in the quenched and tempered (Q+T) condition with a tensile strength of roughly 1100 to 1300 MPa, but it can also be ordered soft annealed, normalized or untreated when the buyer wants to machine first and harden later.
The combination of about 2 % chromium and 2 % nickel gives the grade deep hardenability. Thick plate and heavy round bar sections therefore harden through the full cross section instead of only at the surface, which is what makes the steel suitable for parts working under combined bending, torsion and impact loads.
Chemical Composition of 30CrNiMo8 to EN 10083-3
| Element (%) | C | Si | Mn | P | S | Cr | Mo | Ni |
|---|---|---|---|---|---|---|---|---|
| 30CrNiMo8 | 0.26-0.34 | 0.40 max | 0.50-0.80 | 0.025 max | 0.035 max | 1.80-2.20 | 0.30-0.50 | 1.80-2.20 |
Carbon sets the base hardness that can be reached by quenching. Chromium raises hardenability and wear resistance, molybdenum controls temper embrittlement during high temperature service, and nickel keeps the core tough even in large sections. Sulphur and phosphorus are held to low limits so that fatigue performance is not degraded by inclusions and grain boundary segregation.
Mechanical Properties of Quenched and Tempered 30CrNiMo8
| Thickness (mm) | Min yield strength (MPa) | Tensile strength (MPa) | Min elongation (%) |
|---|---|---|---|
| 3 < t ≤ 8 | 1050 | 1250-1450 | 9 |
| 8 < t ≤ 20 | 1050 | 1250-1450 | 9 |
| 20 < t ≤ 60 | 900 | 1000-1300 | 10 |
| 60 < t ≤ 100 | 800 | 1000-1200 | 11 |
| 100 < t ≤ 160 | 700 | 900-1100 | 12 |
Strength falls as the section grows, because centre cooling is slower and the microstructure coarsens. Designers should select the thickness class that matches the finished part, not the maximum strength value, and should keep in mind that machining stock has to be added to the nominal thickness during ordering.
International Equivalent Grades of 1.6580 Steel
| Standard | EN | DIN / WNr | JIS | AFNOR | BS | GB | GOST | ISO |
|---|---|---|---|---|---|---|---|---|
| Designation | 30CrNiMo8 | 1.6580 | SNCM431 | 30CND8 | 823M30 | 30Cr2Ni2Mo | 3KH3M3F | 31CrNiMo8 |
Equivalent tables are only a starting point for sourcing, because each standard fixes slightly different limits for silicon, phosphorus, sulphur and residuals. For a safety critical component, the chemistry of the actual heat should be compared with the design specification rather than with the table alone.
Heat Treatment Conditions
+A soft annealed: supplied for machining, maximum 248 HB
+N normalized: austenitize at 870-880 °C and cool in air
+QT quenched and tempered: the standard supply condition
+U untreated: as rolled or as forged
Soft annealing: 650-700 °C, then cool at about 10 °C per hour in the furnace
Hardening: 830-860 °C in oil or polymer, or 840-850 °C in water
Stress relieving: hold about 50 °C below the tempering temperature, then cool slowly
Because 30CrNiMo8 is sensitive to hydrogen, heavy sections should be charged into the furnace while still warm and should be tempered immediately after quenching to avoid delayed cracking.
Typical Applications of 30CrNiMo8 Plate and Round Bar
In mechanical manufacturing the steel is used for gears, pinions, connecting rods, spindles, tool holders, moulds and dies, and for bearings, valve bodies, pump parts, wheels, bolts and studs of rotating machinery. Automotive and rail applications include crankshafts, axle shafts, transmission gears and other driveline parts where strength and toughness must coexist.
Aviation, defence, shipbuilding and large structure projects use the grade for shafts, gears, engine components and load carrying plates that see fatigue and wear. In the power sector it is applied to superheater headers of station boilers, turbine and generator parts, and heavy components of power generation equipment where elevated temperature strength and resistance to temper embrittlement are required.
Frequently Asked Questions About 30CrNiMo8 Steel
Q: What does the number 1.6580 mean?
1.6580 is the German material number (Werkstoffnummer) of the grade that EN 10083-3 calls 30CrNiMo8. Both designations describe the same chromium-nickel-molybdenum quenched and tempered steel.
Q: What is the delivery condition of 30CrNiMo8 plate and round bar?
The most common condition is quenched and tempered, which gives a tensile strength of about 1100 to 1300 MPa. Soft annealed, normalized and untreated material can also be supplied when further machining or forming is planned.
Q: Why does the minimum yield strength change with thickness?
Thicker sections cool more slowly during quenching, so the microstructure is coarser. The standard therefore allows a lower minimum yield strength above 20 mm, above 60 mm and above 100 mm.
Q: Can 30CrNiMo8 be welded?
The grade is weldable but requires care: preheating, controlled interpass temperature, suitable low hydrogen consumables and immediate post-weld heat treatment are normally specified for joints that carry structural loads.
Q: Which material can replace 30CrNiMo8 when it is not available?
Depending on the required strength class, designers look at grades such as 34CrNiMo6 or 36NiCrMo16, or at the national equivalents SNCM431, 30CND8, 823M30 and 30Cr2Ni2Mo. Substitution always needs a review of hardenability and toughness.
Q: What sizes are available?
Quenched and tempered plate is usually supplied in thicknesses from about 5 mm to 160 mm, and round bar from about 16 mm to 500 mm diameter, both cut to the sizes required by the final part.